Process method for removing annealing oxide on surface of monocrystalline silicon

By using a process of alkaline washing, hydrofluoric acid immersion, and mixed acid washing, the problem of incomplete removal of oxides from the surface of monocrystalline silicon during annealing was solved, improving production efficiency and reducing acid consumption and cleaning costs.

CN118976746APending Publication Date: 2024-11-19SHANGHAI SHENHE THERMO MAGNETICS ELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411057638.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing technologies cannot completely remove annealing oxides from the surface of monocrystalline silicon in one go, resulting in low production efficiency, high acid consumption, and increased cleaning costs.

Method used

The process involves alkaline washing, hydrofluoric acid immersion, and mixed acid washing. First, residual adhesive and organic matter on the surface of monocrystalline silicon are removed. Then, hydrofluoric acid is used to dissolve silicon dioxide. Finally, annealing oxides are completely removed using mixed acid.

Benefits of technology

It achieves complete removal of oxides on the surface of single-crystal silicon, improves production efficiency, and reduces acid consumption and cleaning costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure HDA0004976892500000011
    Figure HDA0004976892500000011
Patent Text Reader

Abstract

The invention provides a process method for removing annealing oxides on the surface of monocrystalline silicon, and belongs to the technical field of monocrystalline silicon cleaning. The method specifically comprises the following steps: S1, carrying out alkali washing treatment on monocrystalline silicon to remove organic matters such as residual glue on the surface of the monocrystalline silicon; s2, after alkali washing is completed, the monocrystalline silicon is soaked in hydrofluoric acid to remove annealing oxide on the surface of the monocrystalline silicon; and S3, after hydrofluoric acid soaking is finished, acid pickling is performed on the monocrystalline silicon through mixed acid so as to remove residual annealing oxides and impurities on the surface of the monocrystalline silicon. The surface glossiness of the monocrystalline silicon cleaned by the method is high, and an annealing oxide layer on the surface of the monocrystalline silicon can be removed at one time, so that the re-washing rate is reduced, the production efficiency is improved, and meanwhile, the acid consumption and the cleaning cost are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of single crystal silicon cleaning, and in particular to a process for removing annealed oxide on the surface of single crystal silicon. Background Art

[0002] After the single crystal silicon is successfully pulled, the thermal stress generated during the crystal growth process leads to high processing difficulty and low yield, so the crystal rod needs to be stress annealed to eliminate the thermal stress. However, after annealing, a layer of oxide will appear on the crystal rod, which is reddish-brown and attached to the surface of the crystal rod, affecting the quality of the crystal rod.

[0003] At present, mixed acid is usually used to pickle single crystal silicon to remove the annealed oxide on the surface of single crystal silicon. However, when mixed acid is used to pickle the annealed oxide on the surface of single crystal silicon, it cannot be completely corroded at one time. Since the oxide layer of some crystal rods is particularly obvious after annealing and the color is extremely dark, there will still be oxides attached to the surface of the silicon material after pickling and not completely corroded, which makes the surface of the silicon material appear foggy and does not meet the cleaning quality requirements. In addition, the silicon material after pickling is melted back for a second time, and the data of the crystal pulling tracking results shows that it is difficult to pull the crystal, the number of lead-in and release is high, and the whole rod rate is low. Therefore, for such a serious oxide layer, the mixed acid is not completely corroded at one time, and it is generally corroded 2 times or even 3 times... until the oxide layer is completely corroded. However, due to the increase in the number of pickling corrosion times, this process greatly affects the production efficiency, increases the production pressure of the production line, and increases the acid consumption and cleaning costs. Summary of the invention

[0004] In view of this, the present invention provides a process for removing annealing oxide on the surface of single crystal silicon to solve the technical problems that the existing annealing oxide cannot be effectively removed in one go and the production efficiency is low.

[0005] The technical solution adopted by the present invention to solve its technical problem is: A process for removing annealed oxide on the surface of single crystal silicon, specifically comprising the following steps: Step S1, performing alkali washing on the single crystal silicon to remove organic matter such as residual glue on the surface of the single crystal silicon; Step S2: After the alkaline washing is completed, the single crystal silicon is immersed in hydrofluoric acid to remove the annealing oxide on the surface of the single crystal silicon; Step S3: After the hydrofluoric acid immersion is completed, the silicon single crystal is pickled with a mixed acid to remove the remaining annealing oxide and impurities on the surface of the silicon single crystal.

[0006] Preferably, in step S1, alkaline washing treatment of the single crystal silicon includes: placing the single crystal silicon after annealing treatment in alkaline solution for alkaline washing, wherein the ratio of the alkaline solution is: sodium hydroxide: cleaning agent: pure water: defoaming agent = 5-10L: 0.5-5KG: 150-300L: 50-200ML.

[0007] Preferably, the alkali solution temperature is heated to 40-80°C, and the alkali washing time is 2-15 minutes.

[0008] Preferably, in step S2, the alkali-washed single crystal silicon is placed in a hydrofluoric acid soaking tank and soaked for 1-10 minutes in a bubbling state in the soaking tank, wherein the hydrofluoric acid used is 180-200 L of hydrofluoric acid with a content of 49-50%.

[0009] Preferably, in step S3, the ratio of the mixed acid is: hydrofluoric acid: nitric acid = 1-2: 5-10.

[0010] Preferably, the pickling temperature is 20-25°C and the pickling time is 1-5 min.

[0011] Preferably, after step S3, the method further includes: step S4, after the pickling is completed, conventional pure water rinsing is performed at room temperature for 2-10 minutes to remove acid residue on the surface of the single crystal silicon.

[0012] Preferably, after step S4, the method further comprises: step S5, after rinsing, entering into a conventional ultrasonic water washing step, the ultrasonic temperature is maintained at ≥60°C, and the ultrasonic time is controlled at ≥7 minutes.

[0013] Preferably, after step S5, the method further includes: step S6, after the ultrasonic washing is completed, entering the conventional drying stage, using the hot air circulation of the hot air blower, controlling the drying time to be ≥ 25 minutes, and controlling the drying temperature to be between 90°C and 95°C to keep the single crystal silicon dry.

[0014] Preferably, after step S6, the method further includes: step S7, after the drying is completed, entering into a routine packaging inspection to check and confirm whether the annealed oxide layer on the surface of the single crystal silicon is completely corroded.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention first performs alkali washing on the single crystal silicon to remove organic matter such as residual glue on the surface of the single crystal silicon; after the alkali washing, the single crystal silicon is immersed in hydrofluoric acid. Since the annealed oxide on the surface of the single crystal silicon is mainly silicon dioxide, silicon dioxide can be dissolved in hydrofluoric acid, so most of the silicon dioxide on the surface of the single crystal silicon is removed by utilizing the strong corrosiveness of hydrofluoric acid; finally, the single crystal silicon is pickled by mixed acid to completely peel off the annealed oxide on the surface of the single crystal silicon, thereby achieving the purpose of removing the annealed oxide on the surface of the single crystal silicon. The surface of the single crystal silicon cleaned according to the method of the present invention has high glossiness, and the annealed oxide layer on the surface of the single crystal silicon can be removed at one time, thereby reducing the backwashing rate, improving production efficiency, and reducing acid consumption and cleaning costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a diagram showing the effect of removing the oxide layer of the silicon material after alkali washing according to an embodiment of the present invention.

[0017] Figure 2 This is a diagram showing the effect of removing the oxide layer of the silicon material after being soaked in hydrofluoric acid according to an embodiment of the present invention.

[0018] Figure 3 This is a diagram showing the effect of removing the oxide layer of the silicon material after mixed acid pickling according to an embodiment of the present invention.

[0019] Figure 4 This is a diagram showing the effect of removing the oxide layer of the silicon material after alkali washing in the comparative example of the present invention.

[0020] Figure 5 This is a diagram showing the effect of removing the oxide layer of the silicon material after mixed acid pickling in the comparative example of the present invention. DETAILED DESCRIPTION

[0021] The technical solutions and technical effects of the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the present invention.

[0022] Please see Figure 1 A process for removing annealed oxide from the surface of single crystal silicon comprises the following steps: Step S1, performing alkali washing on the single crystal silicon to remove organic matter such as residual glue on the surface of the single crystal silicon; Step S2: After the alkaline washing is completed, the single crystal silicon is immersed in hydrofluoric acid to remove the annealing oxide on the surface of the single crystal silicon; Step S3: After the hydrofluoric acid immersion is completed, the silicon single crystal is pickled with a mixed acid to remove the remaining annealing oxide and impurities on the surface of the silicon single crystal.

[0023] The present invention first performs alkali washing on the single crystal silicon to remove organic matter such as residual glue on the surface of the single crystal silicon; after the alkali washing, the single crystal silicon is immersed in hydrofluoric acid. Since the annealed oxide on the surface of the single crystal silicon is mainly silicon dioxide, silicon dioxide can be dissolved in hydrofluoric acid, so most of the silicon dioxide on the surface of the single crystal silicon is removed by utilizing the strong corrosiveness of hydrofluoric acid; finally, the single crystal silicon is pickled by mixed acid to completely peel off the annealed oxide on the surface of the single crystal silicon, thereby achieving the purpose of removing the annealed oxide on the surface of the single crystal silicon. The surface of the single crystal silicon cleaned according to the method of the present invention has high glossiness, and the annealed oxide layer on the surface of the single crystal silicon can be removed at one time, thereby reducing the backwashing rate, improving production efficiency, and reducing acid consumption and cleaning costs.

[0024] In some embodiments, before step S1, the surface of the single crystal silicon that has completed the annealing treatment is generally marked with a marker pen. Before cleaning, the marking pen marks on the surface of the single crystal silicon can be wiped clean with alcohol.

[0025] In the specific implementation process, the alkali washing treatment of the single crystal silicon includes: placing the single crystal silicon after annealing in an alkali solution for alkali washing, wherein the ratio of the alkali solution is: sodium hydroxide: cleaning agent: pure water: defoaming agent = 5-10L: 0.5-5KG: 150-300L: 50-200ML.

[0026] Furthermore, the alkali solution temperature is heated to 40-80° C., and the alkali washing time is 2-15 minutes.

[0027] Further, in step S2, the alkali-washed single crystal silicon is placed in a hydrofluoric acid soaking tank, and soaked for 1-10 minutes in a bubbling state in the soaking tank, wherein 180-200L of hydrofluoric acid with a content of 49-50% is used. The bubbling of the soaking tank is mainly to enhance the mixing of substances in the liquid and the reaction efficiency through bubbling technology. By using a bubbler, compressed air or steam is introduced into the liquid to generate bubbles, thereby promoting the stirring and mixing of the liquid, so that the hydrofluoric acid and the single crystal silicon can be fully contacted, and the hydrofluoric acid and the annealed oxide on the surface of the single crystal silicon can fully react, so that the annealed oxide is fully dissolved, thereby improving the cleaning efficiency. Furthermore, in step S3, the ratio of the mixed acid is: hydrofluoric acid: nitric acid = 1-2: 5-10. The strong oxidation reaction of nitric acid is used to remove organic matter and metal impurities on the surface of the single crystal silicon, and then hydrofluoric acid is used to remove oxides on the surface of the single crystal silicon.

[0028] Furthermore, the pickling temperature is 20-25°C to ensure a more complete chemical reaction between the mixed acid and the silicon material, and the pickling time is 1-5 min.

[0029] Furthermore, after step S3, the method further includes: step S4, after the pickling is completed, conventional pure water rinsing is performed at room temperature for 2-10 minutes to remove acid residue on the surface of the single crystal silicon.

[0030] Furthermore, after step S4, the method further includes: step S5, after rinsing, entering into a conventional ultrasonic water washing step, the ultrasonic temperature is maintained at ≥60°C, and the ultrasonic time is controlled at ≥7 minutes.

[0031] Furthermore, after step S5, it also includes: step S6, after the ultrasonic water washing is completed, entering the conventional drying stage, using the hot air circulation of the hot air blower, the drying time is controlled to be ≥25 minutes, the drying temperature is controlled between 90°C and 95°C, and the single crystal silicon is kept dry.

[0032] Furthermore, after step S6, the method further includes: step S7, after the drying is completed, entering into a routine packaging inspection to check and confirm whether the annealed oxide layer on the surface of the single crystal silicon is completely corroded.

[0033] For ease of understanding, the present invention is further illustrated by the following examples and comparative examples: Example

[0034] Step 1: For annealed and oxidized silicon material, wipe off the marking pen on the surface of the silicon material with alcohol.

[0035] Step 2: Place the annealed silicon material in an alkaline solution for alkaline washing to remove organic matter such as residual glue; the ratio of the alkaline solution and the specific parameters of the alkaline washing are shown in Table 1. Figure 1 shown.

[0036] Step 3: After alkali washing, the alkali-washed single crystal silicon is placed in a hydrofluoric acid soaking tank and soaked in a bubbling state in the soaking tank; the ratio of hydrofluoric acid and the soaking time are shown in Table 1. Figure 2 shown.

[0037] Step 4: After the hydrofluoric acid soaking, the silicon material is pickled with mixed acid; the ratio of the mixed acid and the specific parameter settings of the pickling are shown in Table 1. Figure 3 shown.

[0038] Step 5: After pickling, rinse with conventional pure water at room temperature for 2-10 minutes to remove the acid residue on the surface of the single crystal silicon.

[0039] Step 6: After rinsing, enter the conventional ultrasonic water washing stage, the ultrasonic temperature is maintained at ≥60℃, and the ultrasonic time is controlled at ≥7 minutes.

[0040] Step 7: After the ultrasonic washing is completed, the conventional drying stage is started, and the hot air circulation is carried out using a hot air blower. The drying time is controlled to be ≥ 25 minutes, and the drying temperature is controlled between 90℃ and 95℃ to keep the single crystal silicon dry.

[0041] Step 8: After drying, enter routine packaging inspection to check and confirm whether the annealed oxide layer on the surface of the single crystal silicon has been completely corroded.

[0042] Table 1

[0043] Comparative Example Compared with the embodiment, the step of hydrofluoric acid soaking is reduced, and the other steps are the same as those of the embodiment. The specific ratios and process parameters are shown in Table 2. The surface of the silicon material after alkali washing is as follows Figure 4 As shown in Figure 2, the surface of the silicon material after pickling is as follows: Figure 5 shown.

[0044] Table 2

[0045] Among them, the surface of the silicon material after cleaning in the embodiment is as follows Figure 3 As shown, the surface of the silicon material after cleaning in the comparative example is as follows Figure 5 As shown, compared Figure 3 and Figure 5 It can be seen that under normal circumstances, alkaline washing + mixed acid pickling cannot completely corrode and remove the oxide layer on the surface of the silicon material, and there are still oxides that have not been completely corroded; but by adding hydrofluoric acid immersion washing and then mixed acid pickling, the oxide layer can be completely corroded and the effect is obvious.

[0046] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A process for removing annealed oxide from the surface of single crystal silicon, characterized in that: The specific steps include: Step S1, performing alkali washing on the single crystal silicon to remove organic matter such as residual glue on the surface of the single crystal silicon; Step S2: After the alkaline washing is completed, the single crystal silicon is immersed in hydrofluoric acid to remove the annealing oxide on the surface of the single crystal silicon; Step S3: After the hydrofluoric acid immersion is completed, the silicon single crystal is pickled with a mixed acid to remove the remaining annealing oxide and impurities on the surface of the silicon single crystal.

2. The process for removing annealed oxide from the surface of single crystal silicon according to claim 1, characterized in that: In step S1, the alkali washing treatment of the single crystal silicon includes: placing the single crystal silicon after annealing in an alkali solution for alkali washing, wherein the ratio of the alkali solution is: sodium hydroxide: cleaning agent: pure water: defoaming agent = 5-10L: 0.5-5KG: 150-300L: 50-200ML.

3. The process for removing annealed oxide from the surface of single crystal silicon according to claim 2, characterized in that: The alkali solution temperature is heated to 40-80°C and the alkali washing time is 2-15 minutes.

4. The process for removing annealed oxide from the surface of single crystal silicon according to claim 1, characterized in that: In step S2, the alkali-washed single crystal silicon is placed in a hydrofluoric acid soaking tank and soaked for 1-10 minutes in a bubbling state in the soaking tank, wherein the hydrofluoric acid used is 180-200 L of hydrofluoric acid with a content of 49-50%.

5. The process for removing annealed oxide from the surface of single crystal silicon according to claim 1, characterized in that: In step S3, the ratio of the mixed acid is: hydrofluoric acid: nitric acid = 1-2: 5-10.

6. The process for removing annealed oxide from the surface of single crystal silicon according to claim 5, characterized in that: The pickling temperature is 20~25℃ and the pickling time is 1-5 min.

7. The process for removing annealed oxide from the surface of single crystal silicon according to claim 1, characterized in that: After step S3, the method further includes: step S4, after the pickling is completed, conventional pure water rinsing is performed at room temperature for 2-10 minutes to remove the acid residue on the surface of the single crystal silicon.

8. The process for removing annealed oxide from the surface of single crystal silicon according to claim 7, characterized in that: After step S4, the method further includes: step S5, after rinsing, entering into a conventional ultrasonic water washing step, the ultrasonic temperature is maintained at ≥60°C, and the ultrasonic time is controlled at ≥7 minutes.

9. The process for removing annealed oxide from the surface of single crystal silicon according to claim 8, characterized in that: After step S5, the process also includes: step S6, after the ultrasonic washing is completed, entering into a conventional drying process, using a hot air blower for hot air circulation, wherein the drying time is controlled to be ≥ 25 minutes, the drying temperature is controlled to be between 90°C and 95°C, and the single crystal silicon is kept dry.

10. The process for removing annealed oxide from the surface of single crystal silicon according to claim 9, characterized in that: After step S6, the method further includes: step S7, after the drying is completed, entering into a routine packaging inspection to check and confirm whether the annealed oxide layer on the surface of the single crystal silicon is completely corroded.

Citation Information

Patent Citations

  • Method for performing recovery treatment on waste layer silicon material

    CN102757051A

  • Mixed acid for cleaning monocrystalline silicon wafer and cleaning method thereof

    CN109560023A

  • Method for cleaning PERC crystalline silicon cell

    CN113990984A

  • Method for cleaning electronic-grade polycrystalline silicon

    CN117443817A

  • Silicon wafer, manufacturing method therefor, and silicon block

    JP2007208060A