Automobile hub bolt trimming-free production process
Through cold heading forming and annealing and tempering, combined with waste heat recovery and cleaning water heating, the problem of high waste and cost in the traditional bolt edge cutting process is solved, and efficient and low-cost production of automobile wheel hub bolts is achieved.
Patent Information
- Application Number
- CN202411180621.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
AI Technical Summary
The traditional automobile hub bolt edge cutting process leads to 5-15% of waste, increasing production costs and affecting the sustainable development of the enterprise.
The screw head and screw parts of the primary molding bolts of cold heading equipment are used, and stress is eliminated through annealing and tempering treatment, combined with waste heat recovery and cleaning water heating, reduce cutting and edge cutting operations, and improve production efficiency and product quality.
The bolts are formed and directional strengthened in one piece, which reduces waste and production costs, improves production efficiency and product consistency, and improves energy utilization efficiency.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile fasteners, in particular to a production process for automobile hub bolts without trimming. Background Art
[0002] Automobile wheel hub bolts are important components that connect automobile wheels and axles. They play the role of fixing and supporting tires, ensuring a safe connection between wheels and axles, and need to have sufficient strength and reliability to withstand various forces and vibrations during vehicle driving.
[0003] Due to the problem of the wheel hub bolt head structure, it is necessary to add a trimming process to ensure the final structure. However, the trimming method will cause about 5-15% of waste, resulting in high production costs and is not conducive to the sustainable development of the enterprise. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a production process for automobile hub bolts without trimming, which solves the problem that the traditional bolt trimming process will cause waste, high production costs, and is not conducive to the sustainable development of the enterprise.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A production process for automobile hub bolts without trimming, comprising the following steps:
[0006] S1. Prepare bolt materials that meet the design requirements and prepare blanks according to the design requirements;
[0007] S2, cold forging is performed by cold forging equipment, and the screw head and screw part of the bolt are formed at one time through the die;
[0008] S3, heating the formed bolts to the annealing temperature, maintaining the temperature for a certain period of time, and cooling after annealing;
[0009] S4, recovering the waste heat of the equipment during annealing and using it for heating the cleaning water;
[0010] S5, using a thread rolling machine to process the screw part to form threads;
[0011] S6. Temper the bolts after thread forming and keep them warm for a certain period of time, then send them into cleaning water for cooling and cleaning.
[0012] Preferably, the bolt material is medium carbon alloy steel.
[0013] Preferably, the cold heading equipment is a hydraulic cold heading machine.
[0014] Preferably, the cold heading forming in step S2 specifically includes the following steps:
[0015] S21, placing the blank in the working area of the cold heading equipment;
[0016] S22, applying pressure downward or upward to the blank by means of a hydraulically driven push device, so that the blank is pressed or stretched through the holes or grooves of the die;
[0017] S23, through the design and arrangement of the mold, the blank is formed into the screw head and the screw part at the same time in a cold heading process;
[0018] S24. After the blank is cold-forging, stop applying pressure and loosen the clamping device of the equipment to remove the formed bolt from the mold.
[0019] Preferably, the annealing temperature is controlled at 800-850° C., the heating time is 7-9 min, and the holding time is 60-70 min.
[0020] Preferably, the annealed bolts are pickled with an acidic solution to remove the surface oxide layer.
[0021] Preferably, the tempering temperature is controlled at 500-550°C, the heating time is 65-70 minutes, and the heat preservation time is 90-95 minutes.
[0022] Preferably, the tempered bolts are cleaned by ultrasonic cleaning, and the cleaning water temperature is 40-50°C.
[0023] Preferably, the cleaning water is heated by recovering waste heat from the annealing equipment through a heat recovery device.
[0024] Preferably, the heat recovery device includes a heat exchanger and a heater.
[0025] The present invention provides a production process for automobile hub bolts without trimming. It has the following beneficial effects:
[0026] 1. The present invention reduces the cutting and trimming operations in the production process by forming the screw head and the screw rod part of the bolt at the same time, thereby improving production efficiency and product consistency, while eliminating the use of trimming molds and saving waste generated by trimming.
[0027] 2. The present invention improves energy utilization efficiency by recovering waste heat generated by the annealing equipment through the waste heat recovery equipment during annealing and using the waste heat recovery equipment to heat cleaning water.
[0028] 3. The trimming-free production process of the present invention realizes one-time forming and directional strengthening of bolts through cold heading and annealing and tempering, reduces cutting and trimming operations, and improves production efficiency and product quality. At the same time, measures such as waste heat recovery and cleaning water heating also improve energy utilization efficiency. This process can be widely used in the production of automobile wheel hub bolts to meet the manufacturing requirements of high quality and high efficiency. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Due to the problem of the wheel hub bolt head structure, it is necessary to add a trimming process to ensure the final structure. However, the trimming method will cause about 5-15% of waste, and the trimming mold loss is relatively large, resulting in high production costs and is not conducive to the sustainable development of the enterprise.
[0031] In order to solve the above problems, the present invention provides a production process for automobile wheel hub bolts without trimming, comprising the following steps:
[0032] Step S1: Prepare bolt material and prepare blank
[0033] First, prepare the bolt material that meets the design requirements, which is medium carbon alloy steel. Then, prepare the bolt blank according to the design requirements, including cutting and processing steps.
[0034] Step S2: Cold heading
[0035] Cold heading is performed using a hydraulic cold heading machine, which has a hydraulic drive system. This step specifically includes the following steps:
[0036] S21: placing the prepared blank in the working area of the cold heading equipment.
[0037] S22: Through the hydraulic drive system, pressure is applied downward or upward to the blank, so that it is pressed or stretched through the holes or grooves of the die. In this process, the design and arrangement of the die allows the blank to form the screw head and screw part at the same time in one cold heading process.
[0038] S23: After the cold heading forming is completed, the pressure is stopped and the clamping device of the equipment is loosened to remove the formed bolt from the mold.
[0039] S24: Remove the cold-forged bolt from the die.
[0040] The function of this cold heading step is to form the bolt head and the screw part at the same time through one-time forming. This process reduces the cutting and trimming operations in the production process, improves production efficiency and product consistency, and eliminates the use of trimming dies, saving waste generated by trimming.
[0041] Step S3: Annealing of bolts
[0042] The formed bolts are heated to the annealing temperature range, kept at a certain temperature for a certain period of time, and then cooled. The specific parameters are that the annealing temperature is controlled at 800-850℃, the heating time is 7-9 minutes, and the insulation time is 60-70 minutes.
[0043] The purpose of annealing is to eliminate stress and hardening during cold heading and to improve the plasticity, strength and toughness of the bolts.
[0044] Step S4: Waste heat recovery
[0045] During annealing, the waste heat recovery equipment recovers the waste heat generated by the annealing equipment and uses it to heat the cleaning water, which can improve energy utilization efficiency.
[0046] Step S5: Processing of the screw part
[0047] The thread rolling machine is used to process the screw part of the bolt to form threads. Thread processing is a common step in bolt manufacturing and is used to connect with other parts.
[0048] Step S6: Tempering and cleaning of bolts
[0049] The bolts after thread forming are tempered and kept at a certain temperature for a certain period of time, and then sent to the cleaning water for cooling and cleaning. The tempering temperature is controlled at 500-550℃, the heating time is 65-70 minutes, and the insulation time is 90-95 minutes. The temperature of the cleaning water is 40-50℃, and the waste heat from the annealing equipment is recovered by the heat recovery equipment for heating.
[0050] Tempering can eliminate the stress in the thread processing process and improve the toughness and corrosion resistance of the bolt. Cleaning is to remove impurities and grease on the surface to ensure product quality.
[0051] In general, the trimming-free production process achieves one-step forming and directional strengthening of bolts through cold heading and annealing and tempering, reduces cutting and trimming operations, and improves production efficiency and product quality. At the same time, measures such as waste heat recovery and washing water heating also improve energy utilization efficiency. This process can be widely used in the production of automobile wheel hub bolts to meet the manufacturing needs of high quality and high efficiency.
[0052] Embodiment 1:
[0053] Step S1: prepare medium carbon alloy steel bolt material and prepare a blank that meets the design requirements.
[0054] Step S2: placing the blank in the working area of the hydraulic cold heading machine, and forming the screw head and the screw rod part simultaneously in one cold heading process through the hydraulic drive system, and then taking the formed bolt out of the mold after winding.
[0055] Step S3: The formed bolt is heated to an annealing temperature of 850° C. and maintained at the temperature for 70 minutes, and then cooled.
[0056] Step S4: recovering the waste heat generated by the equipment during annealing through a heat exchanger and using it to heat cleaning water.
[0057] Step S5: Use a thread rolling machine to process the screw portion to form threads.
[0058] Step S6: Tempering the bolt after thread forming, with the tempering temperature controlled at 500°C, the heating time being 70 minutes, the heat preservation time being 95 minutes, and then ultrasonic cleaning with the cleaning water temperature being 40°C.
[0059] Embodiment 2:
[0060] Step S1: prepare medium carbon alloy steel bolt material and prepare a blank that meets the design requirements.
[0061] Step S2: placing the blank in the working area of the hydraulic cold heading machine, and forming the screw head and the screw rod part simultaneously in one cold heading process through the hydraulic drive system, and then taking the formed bolt out of the mold after winding.
[0062] Step S3: The formed bolt is heated to an annealing temperature of 800° C. and maintained at the temperature for 60 minutes, and then cooled.
[0063] Step S4: recovering the waste heat generated by the equipment during annealing through a heat exchanger and using it to heat cleaning water.
[0064] Step S5: Use a thread rolling machine to process the screw portion to form threads.
[0065] Step S6: Tempering the bolt after thread forming, with the tempering temperature controlled at 550°C, the heating time being 65 minutes, the heat preservation time being 90 minutes, and then ultrasonic cleaning with the cleaning water temperature being 50°C.
[0066] Embodiment three:
[0067] Step S1: prepare medium carbon alloy steel bolt material and prepare a blank that meets the design requirements.
[0068] Step S2: placing the blank in the working area of the hydraulic cold heading machine, and forming the screw head and the screw rod part simultaneously in one cold heading process through the hydraulic drive system, and then taking the formed bolt out of the mold after winding.
[0069] Step S3: The formed bolt is heated to an annealing temperature of 830° C. and maintained at the temperature for 65 minutes, and then cooled.
[0070] Step S4: recovering the waste heat generated by the equipment during annealing through a heat exchanger and using it to heat cleaning water.
[0071] Step S5: Use a thread rolling machine to process the screw portion to form threads.
[0072] Step S6: Tempering the bolts after thread forming, with the tempering temperature controlled at 520°C, the heating time being 68 minutes, the heat preservation time being 93 minutes, and then ultrasonic cleaning with the cleaning water temperature being 45°C.
[0073] Embodiment 4:
[0074] Step S1: prepare medium carbon alloy steel bolt material and prepare a blank that meets the design requirements.
[0075] Step S2: placing the blank in the working area of the hydraulic cold heading machine, and forming the screw head and the screw rod part simultaneously in one cold heading process through the hydraulic drive system, and then taking the formed bolt out of the mold after winding.
[0076] Step S3: The formed bolt is heated to an annealing temperature of 840° C. and maintained at the temperature for 60 minutes, and then cooled.
[0077] Step S4: recovering the waste heat generated by the equipment during annealing through a heat exchanger and using it to heat cleaning water.
[0078] Step S5: Use a thread rolling machine to process the screw portion to form threads.
[0079] Step S6: Tempering the bolt after thread forming, with the tempering temperature controlled at 510°C, the heating time being 65 minutes, the heat preservation time being 90 minutes, and then ultrasonic cleaning with the cleaning water temperature being 42°C.
[0080] Embodiment five:
[0081] Step S1: prepare medium carbon alloy steel bolt material and prepare a blank that meets the design requirements.
[0082] Step S2: placing the blank in the working area of the hydraulic cold heading machine, and forming the screw head and the screw rod part simultaneously in one cold heading process through the hydraulic drive system, and then taking the formed bolt out of the mold after winding.
[0083] Step S3: The formed bolt is heated to an annealing temperature of 820° C. and maintained at the temperature for 60 minutes, and then cooled.
[0084] Step S4: recovering the waste heat generated by the equipment during annealing through a heat exchanger and using it to heat cleaning water.
[0085] Step S5: Use a thread rolling machine to process the screw portion to form threads.
[0086] Step S6: Tempering the bolts after thread forming, with the tempering temperature controlled at 530°C, the heating time being 70 minutes, the heat preservation time being 90 minutes, and then ultrasonic cleaning with the cleaning water temperature being 48°C.
[0087] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for automobile hub bolts without trimming, characterized in that: The following steps are involved: S1. Prepare bolt materials that meet the design requirements and prepare blanks according to the design requirements; S2, cold forging is performed by cold forging equipment, and the screw head and screw part of the bolt are formed at one time through the die; S3, heating the formed bolts to the annealing temperature, maintaining the temperature for a certain period of time, and cooling after annealing; S4, recovering the waste heat of the equipment during annealing and using it for heating the cleaning water; S5, using a thread rolling machine to process the screw part to form threads; S6. Temper the bolts after thread forming and keep them warm for a certain period of time, then send them into cleaning water for cooling and cleaning.
2. The process for producing automobile hub bolts without trimming according to claim 1, characterized in that: The bolt material is medium carbon alloy steel.
3. The process for producing automobile hub bolts without trimming according to claim 1, characterized in that: The cold heading equipment is a hydraulic cold heading machine.
4. The process for producing automobile hub bolts without trimming according to claim 3, characterized in that: The cold heading forming in step S2 specifically includes the following steps: S21, placing the blank in the working area of the cold heading equipment; S22, applying pressure downward or upward to the blank by means of a hydraulically driven push device, so that the blank is pressed or stretched through the holes or grooves of the die; S23, through the design and arrangement of the mold, the blank is formed into the screw head and the screw part at the same time in a cold heading process; S24. After the blank is cold-forging, stop applying pressure and release the clamping device of the equipment to remove the formed bolt from the mold.
5. The process for producing automobile hub bolts without trimming according to claim 1, characterized in that: The annealing temperature is controlled at 800-850° C., the heating time is 7-9 minutes, and the heat preservation time is 60-70 minutes.
6. The process for producing automobile hub bolts without trimming according to claim 5, characterized in that: The annealed bolts are pickled with an acid solution to remove the surface oxide layer.
7. The process for producing automobile hub bolts without trimming according to claim 1, characterized in that: The tempering temperature is controlled at 500-550°C, the heating time is 65-70 minutes, and the heat preservation time is 90-95 minutes.
8. The process for producing automobile hub bolts without trimming according to claim 1, characterized in that: The tempered bolts are cleaned by ultrasonic wave, and the cleaning water temperature is 40-50°C.
9. The process for producing automobile hub bolts without trimming according to claim 8, characterized in that: The cleaning water is heated by recovering waste heat from the annealing equipment through a heat recovery device.
10. The process for producing automobile hub bolts without trimming according to claim 9, characterized in that: The heat recovery device includes a heat exchanger and a heater.