Preparation method of automobile brake disc
Through the method of combining mold and melt furnace, the airflow pressure and holding time are controlled, and the problems of poor formability and inconsistent interface of ceramic-enhanced aluminum-based composite materials are solved, and the compactness and crack-free preparation of the automobile brake disc are achieved. Braking performance requirements.
Patent Information
- Application Number
- CN202411082631.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
When preparing automobile brake discs in traditional powder metallurgy processes, the ceramic-reinforced aluminum-based composite material has poor formability, the interface between the disc cap and the disc body is inconsistent and cracks are prone to occur, making it difficult to meet the braking performance requirements.
By combining mold and melt furnace, the melt of ceramic-reinforced aluminum-based composite material is introduced into the mold cavity by controlling the airflow pressure and holding time, and cooled and released to ensure the consistency and compactness of the interface between the disc cap and the disc body. , avoid cracks.
It realizes the compactness and crack-free preparation of the automobile brake disc, meets the braking performance requirements, and improves the appearance integrity and interface consistency of the product.
Smart Images

Figure CN118976883A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brake disc preparation, in particular to a method for preparing an automobile brake disc. Background Art
[0002] Lightweighting is one of the most effective means to achieve energy conservation and consumption reduction for automobiles and other transportation vehicles. Using high-performance light metal materials instead of steel materials in key moving parts such as engines and brake discs of transportation equipment can not only reduce the weight of the entire vehicle and reduce the momentum of high-speed moving parts of transportation equipment, but also significantly improve the dynamic performance of transportation equipment while reducing energy consumption.
[0003] Ceramic-reinforced aluminum-based composite materials have low density, high specific strength and specific stiffness, high thermal conductivity, and excellent wear resistance and corrosion resistance, and have broad application prospects in the field of lightweight structural parts. Specifically applied to brake discs, since the disc body needs to have high temperature resistance, wear resistance and other properties, and the disc cap needs to have relatively high mechanical properties, the disc body uses a high volume fraction of ceramic-reinforced aluminum-based composite materials, and the disc cap uses a low volume fraction of ceramic-reinforced aluminum-based composite materials to meet their respective performance requirements. However, when the above-mentioned brake discs are prepared using traditional powder metallurgy processes, the two powder materials are easy to penetrate each other during the powder filling and pressing process, resulting in an elliptical or even completely irregular interface between the disc body and the disc cap. In addition, considering that the formability of ceramic reinforced aluminum-based composites deteriorates due to the addition of ceramic reinforcement phase, simple green billets are usually pressed out first, such as annular or cylindrical green billets, which are then sintered and forged to form the overall structure of the brake disc, such as a disc cap with a gooseneck structure, and finally machined into the final product. However, the flow of materials during the forging process is difficult to control and cracks are prone to appear on the outside of the disc cap. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing an automobile brake disc, which can ensure that even if the disc cap and the disc body are made of different materials, their interfaces remain consistent, and the prepared brake disc has good density and no cracks, meeting the braking requirements.
[0005] A method for preparing an automobile brake disc, the automobile brake disc comprising an annular disc body and a disc cap, the disc cap comprising an end, a side wall extending axially along the end, and a connecting portion extending radially along the side wall, the method for preparing the automobile brake disc comprising the following steps:
[0006] Providing the annular disk body;
[0007] A mold is provided, wherein the mold comprises an upper mold, a lower mold and a female mold which are coaxially arranged. After the molds are closed, the upper mold and the lower mold are enclosed in the female mold to form a mold cavity, wherein the mold cavity comprises a first part and a second part which are interconnected, wherein the first part is adapted to the annular disk body, and the second part is adapted to the disk cap to be formed, and a cooling device is provided in the part of the upper mold used for forming the disk cap;
[0008] A melt furnace is provided, the melt furnace comprises a furnace body and a riser pipe, one end of the riser pipe is located in the furnace body, and the other end passes through the center of the lower mold and communicates with the mold cavity; a ceramic reinforced aluminum-based composite material melt is contained in the furnace body;
[0009] The annular disc body is placed in the first part of the mold cavity, preheated to 200°C to 250°C after the mold is closed, the cooling device is started, the air flow pressure entering the furnace body is controlled to be 0.05MPa to 0.15MPa, the ceramic reinforced aluminum-based composite material melt is compressed to enter the mold cavity through the riser pipe, and after maintaining the pressure for 10s to 25s, the pressure is released, cooled, demolded, and machined to obtain an automobile brake disc.
[0010] In one of the embodiments, the diameter of the riser pipe at the connection point with the mold cavity is 50 mm to 70 mm.
[0011] In one embodiment, the portion of the upper die used to form the end portion is 20 mm to 30 mm thick; the portion of the upper die used to form the side wall is 15 mm to 25 mm thick.
[0012] In one embodiment, the annular disc body includes an outer ring part and an inner ring part, the outer ring part is used for friction braking with the brake pad, the inner ring part is used for engaging with the disc cap, and the thickness of the inner ring part is less than the thickness of the outer ring part.
[0013] In one of the embodiments, the inner ring portion has a plurality of axial through holes evenly distributed along the circumferential direction, and the diameter of each of the axial through holes is 8 mm to 16 mm.
[0014] In one embodiment, the ceramic reinforced aluminum-based composite material melt is composed of 10% to 20% ceramic reinforced particles and the remainder aluminum alloy, the annular disk is prepared from 35% to 55% ceramic reinforced aluminum-based composite material and the remainder aluminum alloy, and the aluminum alloy is selected from at least one of the second series aluminum alloy, the fourth series aluminum alloy and the sixth series aluminum alloy.
[0015] In one of the embodiments, the temperature of the ceramic reinforced aluminum-based composite material melt is 700°C to 740°C.
[0016] In one embodiment, the cooling temperature is below 100°C.
[0017] In one of the embodiments, the height of the side wall of the disk cap is 10 mm to 35 mm.
[0018] In one embodiment, the height of the side wall of the disk cap is greater than 35 mm, and a densification step is also included between the demoulding and machining steps.
[0019] The above-mentioned method for preparing the automobile brake disc controls the air flow pressure to introduce the ceramic reinforced aluminum-based composite material melt into the mold cavity where the annular disc body is placed. Under the action of the cooling device, the melt gradually solidifies from the end in contact with the disc body to the end away from the disc body. By controlling the holding time, on the one hand, it is ensured that the melt fills the entire mold cavity and solidifies completely, and on the other hand, it can effectively reduce the shrinkage holes generated during the casting process and improve the density of the product.
[0020] In addition, since the annular disk is already a finished product, its edge is relatively stable, and the melt solidifies after contacting it without affecting the edge, thereby ensuring the consistency of the interface.
[0021] The automobile brake disc prepared by the above method has an intact appearance without cracks and meets the braking performance required by existing automobile brake discs. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the connection structure of a mold and a melt furnace in one embodiment. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0024] It should be noted that when an element is referred to as being "disposed" on another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0026] A method for preparing a brake disc for an automobile according to an embodiment of the present invention comprises the following steps S110 to S130:
[0027] S110, providing an annular disk body.
[0028] The annular disc body comprises an outer ring part and an inner ring part, wherein the thickness of the inner ring part is less than the thickness of the outer ring part. The outer ring part is used for friction braking with the brake pad, and the inner ring part is used for engaging with the disc cap.
[0029] It can be understood that the inner ring portion can be a continuous inner ring, or an inner ring composed of a plurality of protrusions that are evenly spaced along the circumferential direction and extend radially.
[0030] In order to meet the friction braking requirements, the annular disc body is prepared from 35% to 55% of ceramic reinforcement particles and the remainder of aluminum alloy. The aluminum alloy is selected from at least one of the second series aluminum alloy, the fourth series aluminum alloy and the sixth series aluminum alloy.
[0031] It should be noted that the annular disc body of the present application can be prepared from the above-mentioned materials using a powder metallurgy process, or can be prepared using an infiltration process, as long as it can meet the requirements of friction braking.
[0032] Furthermore, the inner ring portion is evenly distributed with a plurality of axial through holes along the circumferential direction, and the aperture of each axial through hole is 8 mm to 16 mm. It can be understood that if the inner ring portion is an inner ring composed of a plurality of protrusions evenly spaced along the circumferential direction and extending radially, the above-mentioned axial through holes are arranged one by one on each protrusion.
[0033] By setting axial through holes, the subsequent ceramic reinforced aluminum-based composite material melt flows into these through holes and solidifies. The solidified melt completely wraps the inner ring part of the disk body, which can effectively improve the connection strength between the disk body and the disk cap.
[0034] S120, provide Figure 1 A mold 10 and a melt furnace 20 are shown.
[0035] The mold 10 includes an upper mold 12, a lower mold 14 and a female mold 16 which are coaxially arranged. After the molds are closed, the upper mold 12 and the lower mold 14 are enclosed in the female mold 16 to form a mold cavity. The mold cavity includes a first portion 102 and a second portion 104 which are connected to each other, wherein the first portion 102 is adapted to the annular disk body, and the second portion 104 is adapted to the disk cap to be formed.
[0036] Further, a cooling device 18 is provided in the portion of the upper mold 12 for forming the disk cap. Further, the cooling device 18 is a circulating cooling water pipe.
[0037] In this embodiment, the disk cap includes an end, a side wall extending axially along the end, and a connecting portion extending radially along the side wall. The portion of the upper die 12 used to form the end is 20 mm to 30 mm thick. The portion of the upper die 12 used to form the side wall is 15 mm to 25 mm thick.
[0038] By providing a cooling device 18 in the portion of the upper mold 12 used for forming the disk cap, the temperature in the mold cavity can be gradually reduced.
[0039] Furthermore, the melt furnace 20 includes a furnace body 22 and a riser pipe 24 , wherein one end of the riser pipe 24 is located in the furnace body 22 , and the other end passes through the center of the lower mold 14 and communicates with the mold cavity.
[0040] Furthermore, an air inlet 222 and a pressure relief port 224 are provided on the top of the furnace body 22. During casting, the pressure relief port 224 is closed, and the air flow is controlled to enter the furnace body 22 from the air inlet 222, and the compressed melt enters the mold cavity through the riser 24; after casting, the air inlet 222 is closed and the pressure relief port 224 is opened for pressure relief.
[0041] In this embodiment, the furnace body 22 is filled with a ceramic-reinforced aluminum-based composite melt at 700° C. to 740° C. The ceramic-reinforced aluminum-based composite melt is composed of 10% to 20% ceramic-reinforced particles and the remainder of aluminum alloy. The aluminum alloy is selected from at least one of a second series aluminum alloy, a fourth series aluminum alloy, and a sixth series aluminum alloy.
[0042] The ceramic reinforced aluminum-based composite material melt of the above special composition can meet the performance requirements of the brake disc cap structure on the one hand, and facilitate the machining of excess solidified melt, such as the solidified melt at the center hole position of the disc cap end on the other hand.
[0043] In this embodiment, the diameter of the riser pipe 24 at the point where it communicates with the mold cavity is 50 mm to 70 mm.
[0044] S130, place the annular disc body in the first part 102 of the mold cavity, preheat it to 200℃~250℃ after mold closing, start the cooling device 18, control the air flow pressure into the furnace body 22 to 0.05MPa~0.15MPa, and compress the ceramic reinforced aluminum-based composite material melt into the mold cavity through the riser pipe. After maintaining the pressure for 10s~25s, release the pressure, cool, demold, and machine to obtain the automobile brake disc.
[0045] The gas flow is an inert gas flow, such as argon, nitrogen, etc., to prevent the melt from being oxidized and affecting the bonding with the disc body.
[0046] Place the annular disk in the first part of the mold cavity and preheat the mold to 200℃~250℃, then start the cooling device and introduce high-temperature melt at the same time. On the one hand, it can effectively remove the water vapor adsorbed on the mold surface to avoid the formation of pores on the workpiece surface during casting, and on the other hand, it can prevent the high-temperature melt from directly contacting the cooling disk and the mold wall, causing cracks.
[0047] By controlling the air flow pressure to 0.05MPa~0.15MPa and the holding time to 10s~25s, it can not only ensure that the melt fills the entire mold cavity and solidifies completely, but also effectively reduce the shrinkage holes generated during the casting process and improve the density of the product, thereby ensuring that the excess solidified melt can be removed by machining after subsequent demoulding without the need for forging to densify.
[0048] Furthermore, the cooling temperature is below 100° C. Demolding after cooling can effectively avoid deformation of the disc body material and the disc cap material due to inconsistent thermal expansion coefficients.
[0049] The above method can be used to prepare automobile brake discs with a disc cap side wall height of 10mm to 35mm. Without forging to be dense, an automobile brake disc with high density and no cracks that meets braking requirements can be obtained.
[0050] If the side wall height of the disc cap exceeds 35mm, it is necessary to perform forging and densification after demolding and before machining to further improve the density of the brake disc.
[0051] The preparation method of the above-mentioned automobile brake disc controls the temperature of the melt to 700℃~740℃, the thickness of the part of the upper mold 12 used for forming the end is 20mm~30mm, the thickness of the part of the upper mold 12 used for forming the side wall is 15mm~25mm, and then the diameter of the pipe at the connection between the riser pipe 24 and the mold cavity is controlled to be 50mm~70mm, and the air flow pressure entering the melt furnace 20 is controlled to be 0.05MPa~0.15MPa, and the holding time is 10s~25s. All aspects work together to make the melt just fill the entire mold cavity and solidify completely, and can effectively reduce the shrinkage holes generated during the casting process and improve the density of the product.
[0052] The following are specific embodiments.
[0053] Example 1
[0054] An automobile brake disc with a disc cap side wall height of 35 mm is prepared by adopting steps such as steps S110 to S130, the temperature of the melt is controlled to 700°C, the portion of the upper mold 12 used to form the end is 20 mm thick, the portion of the upper mold 12 used to form the side wall is 15 mm thick, the diameter of the riser 24 connected to the mold cavity is 50 mm, the air flow pressure entering the melt furnace 20 is 0.05 MPa, and the holding time is 10 s. Thus, an automobile brake disc with high density, intact appearance, no cracks, and good interface consistency can be obtained.
[0055] Comparative Example 1
[0056] Comparative Example 1 is substantially the same as Example 1, except that the air flow pressure into the melt furnace 20 is 0.03 MPa. After demoulding, microcracks exist at the connection position between the friction layer and the structural layer on the back side of the disc cap, and the cracks cannot be completely removed by machining, so the brake disc is unqualified.
[0057] Example 2
[0058] An automobile brake disc with a disc cap side wall height of 30 mm is prepared by adopting steps such as steps S110 to S130, the temperature of the melt is controlled to be 740°C, the portion of the upper mold 12 used for forming the end is 30 mm thick, the portion of the upper mold 12 used for forming the side wall is 25 mm thick, the diameter of the riser 24 connected to the mold cavity is 70 mm, the air flow pressure entering the melt furnace 20 is 0.15 MPa, and the holding time is 25 s. An automobile brake disc with a good appearance, no cracks, and good interface consistency can be obtained.
[0059] Comparative Example 2
[0060] Comparative Example 2 is substantially the same as Example 2, except that the air flow pressure into the melt furnace 20 is 0.03 MPa. After demoulding, microcracks exist at the connection position between the friction layer and the structural layer on the back side of the disc cap, and the cracks cannot be completely removed by machining, so the brake disc is unqualified.
[0061] Example 3
[0062] An automobile brake disc with a disc cap side wall height of 45 mm is prepared by adopting steps such as steps S110 to S130, and forging is performed to make it dense after demolding but before machining. The temperature of the melt is controlled to be 720°C, the thickness of the portion of the upper die 12 used for forming the end is 25 mm, the thickness of the portion of the upper die 12 used for forming the side wall is 20 mm, the diameter of the riser pipe 24 connected to the mold cavity is 60 mm, the air flow pressure entering the melt furnace 20 is 0.10 MPa, and the holding time is 20 s. Thus, an automobile brake disc with a good appearance, no cracks, and good interface consistency can be obtained.
[0063] Comparative Example 3
[0064] Comparative Example 3 is substantially the same as Example 3, except that the forging step is omitted. As a result, the brake disc fails the bench test.
[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a brake disc for an automobile, wherein the brake disc for an automobile comprises an annular disc body and a disc cap, wherein the disc cap comprises an end portion, a side wall extending axially along the end portion, and a connecting portion extending radially along the side wall, wherein: The method for preparing the automobile brake disc comprises the following steps: Providing the annular disk body; A mold is provided, wherein the mold comprises an upper mold, a lower mold and a female mold which are coaxially arranged. After the molds are closed, the upper mold and the lower mold are enclosed in the female mold to form a mold cavity, wherein the mold cavity comprises a first part and a second part which are interconnected, wherein the first part is adapted to the annular disk body, and the second part is adapted to the disk cap to be formed, and a cooling device is provided in the part of the upper mold used for forming the disk cap; A melt furnace is provided, the melt furnace comprises a furnace body and a riser pipe, one end of the riser pipe is located in the furnace body, and the other end passes through the center of the lower mold and communicates with the mold cavity; a ceramic reinforced aluminum-based composite material melt is contained in the furnace body; The annular disc body is placed in the first part of the mold cavity, preheated to 200°C to 250°C after the mold is closed, the cooling device is started, the air flow pressure entering the furnace body is controlled to be 0.05MPa to 0.15MPa, the ceramic reinforced aluminum-based composite material melt is compressed to enter the mold cavity through the riser pipe, and after maintaining the pressure for 10s to 25s, the pressure is released, cooled, demolded, and machined to obtain an automobile brake disc.
2. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The diameter of the riser pipe at the point where it communicates with the mold cavity is 50 mm to 70 mm.
3. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The thickness of the portion of the upper die used to form the end portion is 20 mm to 30 mm; the thickness of the portion of the upper die used to form the side wall is 15 mm to 25 mm.
4. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The annular disc body comprises an outer ring part and an inner ring part, wherein the outer ring part is used for friction braking with a brake pad, and the inner ring part is used for engaging with the disc cap, and the thickness of the inner ring part is smaller than that of the outer ring part.
5. The method for preparing a brake disc for an automobile according to claim 4, characterized in that: The inner ring part is uniformly provided with a plurality of axial through holes along the circumferential direction, and the diameter of each axial through hole is 8 mm to 16 mm.
6. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The ceramic reinforced aluminum-based composite material melt is composed of 10% to 20% ceramic reinforced particles and the remainder aluminum alloy, the annular disk is prepared from 35% to 55% ceramic reinforced particles and the remainder aluminum alloy, and the aluminum alloy is selected from at least one of the second series aluminum alloy, the fourth series aluminum alloy and the sixth series aluminum alloy.
7. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The temperature of the ceramic reinforced aluminum-based composite material melt is 700°C to 740°C.
8. The method for preparing a vehicle brake disc according to claim 1, characterized in that: The cooling temperature is below 100°C.
9. The method for preparing a vehicle brake disc according to any one of claims 1 to 8, characterized in that: The height of the side wall of the disk cap is 10 mm to 35 mm.
10. The method for preparing a vehicle brake disc according to any one of claims 1 to 8, characterized in that: The height of the side wall of the disk cap is greater than 35 mm, and a densification step is also included between the demoulding and machining steps.
Citation Information
Patent Citations
Automobile brake disc and manufacturing method thereof
CN105041921A
Wear-resisting material, local enhanced light metal base composite material and preparing method
CN107876730A
Brake disc and preparation method thereof
CN107917160A
Hybrid lightweight brake disk and production method
CN108331863A
Aluminum-based composite solid brake disc for automobile and preparation method of aluminum-based composite solid brake disc
CN112780708A