Simple and high-quality laser welding method for aluminum-silicon coating hot-formed ultrahigh-strength steel
By entering the aluminum-silicon plating ultra-high strength steel welding point and controlling the laser welding parameters, the aggregation problem of plating in the weld is solved, the joint strength is improved, and high-quality welding effect is achieved, and the laser welding parameters are simplified. The process flow and reduce costs.
Patent Information
- Application Number
- CN202411102978.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
AI Technical Summary
In automobile manufacturing, during the laser welding process of aluminum-silicon plating, the plating is easy to enter the weld, resulting in low joint strength, the existing solutions are complex and increase production costs, and it is not possible to effectively solve the plating in the weld seam. aggregation problem in.
By passing the mixed gas composed of argon (Ar) and nitrogen (N2) into the welding point, the gas flow rate and angle are controlled, and the laser welding parameters are adjusted, the aggregation degree of plating in the weld is reduced and austenite structure is promoted. to improve joint strength.
High-strength overlap joints are realized, process flow is simplified, implementation costs are reduced, the need to remove plating and attach processing steps is avoided, and welding quality is significantly improved.
Smart Images

Figure CN118976991A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of laser welding, and in particular relates to a simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating. Background Art
[0002] According to statistics from the China Association of Automobile Manufacturers, my country's automobile production and sales will reach 30.161 million and 30.094 million respectively in 2023, up 11.6% and 12% year-on-year respectively, and both annual production and sales will hit record highs. Among them, the sales volume of fuel vehicles accounts for nearly half of the automobile sales share, which brings the dual challenges of resources and environmental issues. How to reduce the fuel consumption of fuel vehicles and achieve carbon neutrality is one of the main issues at this stage. In order to achieve this goal, while ensuring the quality and service life of the car, automakers need to design the car to reduce weight. Studies have shown that for every 100kg weight loss of the car, the fuel car can save about 0.3 to 0.5L of fuel per 100 kilometers; while the cruising range of electric vehicles can be increased by about 15Km. In addition, car weight reduction can significantly increase the service life of tires and reduce the manufacturing costs of enterprises.
[0003] Hot-formed steel (PHS) is an alloy steel containing trace amounts of boron. After being heated in a furnace, it is transferred to a closed mold for quenching and forming (the cooling rate must exceed 30°C / s). Its maximum tensile strength can exceed 1500MPa. Hot-formed ultra-high-strength steel is already one of the most widely used materials for lightweight automobiles, with a production scale of about 50 billion.
[0004] Automotive companies face two major challenges in welding hot-formed ultra-high-strength steel. First, after welding hot-formed steel, a softening zone is likely to appear at the joint. Second, in order to prevent decarburization and oxidation of the steel during hot stamping, it is necessary to coat the surface with a coating, usually an aluminum-silicon coating. During the welding process, the coating melts and enters the weld, which causes the mechanical properties of the joint to deteriorate, to the point that the strength is far lower than that of the parent material. There has been no perfect solution to the latter problem so far. Therefore, how to eliminate the negative effects of the coating to fully improve the quality of welded hot-formed steel joints is the key to the lightweighting process of automobiles.
[0005] At present, there are three main technologies used by automobile companies to weld hot-formed steel: resistance spot welding, arc welding and laser welding. Resistance spot welding has high requirements on the shape and size of the workpiece and requires precise control of welding parameters (such as welding current, welding time, electrode pressure); the heat input during arc welding is too large, and the weld is prone to Widmanstätten structure and softening of the heat-affected zone. Compared with resistance spot welding and argon arc welding, laser welding has the advantages of high precision, low heat input, small heat-affected zone and high joint strength. It is a non-contact welding method that can effectively avoid the wear of resistance spot welding electrodes, and has no restrictions on the size and size of the material. It is an excellent welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating.
[0006] For the laser welding of hot-formed ultra-high-strength steel with aluminum-silicon coating, during the welding process, since the Al-Si coating easily enters the weld, segregation will occur in local areas, forming high-temperature ferrite (δ phase) with poor plasticity and toughness. Cracks are easily generated and extended in the δ phase, resulting in very low joint strength, which seriously affects the application of the parent material. At present, laser cleaning, mechanical grinding, shot peening and other technologies are usually used to remove the coating before welding. However, this method will increase the cost of production and manufacturing, and sometimes even cause certain damage to the steel matrix, which will bring some new problems. It is not an efficient and applicable method. In addition, some researchers have taken a different approach and used filler metal to control the organization, such as using Ni or Cr foil or wire to place in the gap of the butt joint to generate more martensite in the joint, thereby improving the joint strength, or using (C powder + Fe powder) alloy powder to fill the lap weld to reduce the ferrite content, or using nickel foil or powder, or wire to fill the lap weld to reduce the ferrite content. The starting point of the above technologies is to add austenite stabilizing elements such as Ni and C to the weld, so that the weld generates more austenite phase during the high temperature process, thereby reducing the generation and aggregation of high temperature ferrite (δ phase). However, adding wire, foil, alloy, etc. will increase the process and manufacturing difficulty. For this reason, it is urgent to provide a simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating. Summary of the invention
[0007] In view of the problems existing in the above-mentioned prior art, the present invention provides a simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating. The process is simple and has low implementation cost. It does not require removal of the coating on the steel surface, nor does it require the use of complex laser welding processes with additional steps. Only by introducing special-purpose gas components into the welding point and controlling the laser parameters, the weld structure can be optimized to achieve the purpose of improving the joint strength.
[0008] In order to achieve the above object, the present invention provides a simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating, comprising the following steps:
[0009] Step 1: pre-treat the double-sided aluminum-silicon coated hot-formed ultra-high-strength steel plate, overlap the welding parts of the two aluminum-silicon coated hot-formed ultra-high-strength steel plates, and fix them on the welding platform with a welding fixture;
[0010] Step 2: Use a vent pipe to output a specially selected gas that can promote the formation of more austenite structure in the weld to the welding pool; the specially selected gas is a mixed gas composed of Ar and N2;
[0011] Step 3: Start the laser welding system, melt the base material by laser to perform welding, and form a weld after cooling; during the welding process, adjust the ratio and flow of the selected gas, and control the laser process parameters, and reduce the aggregation of the coating in the weld by adjusting the weld structure to obtain a higher strength lap joint; wherein, the gas flow rate of the selected gas is 20-30L / min, and the angle between the vent pipe and the weld is 30-60°; wherein, the incident angle of the laser is 85-90°, the laser power is 2-4kW, and the welding speed is 1-3m / min.
[0012] In order to improve the cleaning effect and fully ensure the subsequent welding quality, the pretreatment method in step 1 is as follows:
[0013] First, use a cotton ball dipped in an organic solvent to wipe the front and back surfaces of the aluminum-silicon coated hot-formed ultra-high-strength steel plate to remove surface impurities; then quickly blow dry the wiped aluminum-silicon coated hot-formed ultra-high-strength steel plate, and then place it in a dry place for welding.
[0014] Preferably, the organic solvent is acetone.
[0015] Furthermore, in order to strictly control the content of alloy elements to obtain a weld with better tensile strength, in step three, the volume percentage content of N2 in the selected gas is 90% to 40%.
[0016] Preferably, in step one, the thickness of the aluminum-silicon coated hot-formed ultra-high strength steel is 0.5 to 3.5 mm, and the thickness of the aluminum-silicon coating in the aluminum-silicon coated hot-formed ultra-high strength steel is 30 to 70 μm.
[0017] Furthermore, in order to better reduce the degree of aggregation of the coating at the fusion line so as to obtain a lap joint with higher strength, in step three, the volume percentage content of N2 in the selected gas is 70%, the gas flow rate is 25L / min, and the angle between the vent pipe and the weld is 45°; in step three, the incident angle of the laser is 85°, the laser power is 3kW, and the welding speed is 1m / min.
[0018] In the present invention, by pretreatment, impurities such as oil stains on the surface of aluminum-silicon coated hot-formed ultra-high-strength steel can be effectively removed, which is conducive to ensuring the subsequent welding quality. By controlling the laser process and coordinating the protection of special gases, the weld structure can be effectively adjusted, the aggregation degree of the coating in the weld can be reduced, especially the aggregation degree of the coating at the fusion line is reduced, thereby obtaining a higher strength lap joint. After thousands of experiments, it was found that in addition to austenite stabilizing elements such as Ni and C, N is also a strong austenitizing stabilizing element, and the addition method of N can be added without presetting. Its addition method is relatively special. Since a protective gas is introduced into the molten pool during welding, N can be mixed in the protective gas as N2 gas (the commonly used protective gas for laser welding steel is argon). Using Ar+N2 mixed gas to the molten pool, N can enter the weld in a non-contact form. According to the basic theory of materials science and welding metallurgy, the high-temperature molten pool can absorb a large amount of N, and then the amount of N dissolved can be guaranteed. Controlling the amount of N dissolved is mainly solved by changing the proportion of the mixed gas and the gas flow rate. Therefore, the performance of welded joints can be improved simply and effectively through this non-contact method of adding alloying elements.
[0019] The present invention can dissolve the austenitized alloying element N into the weld in a non-contact manner by passing a gas containing N into the weld, which not only simplifies the method of adding alloying elements, but also can conveniently strictly control the content of alloying elements by controlling the gas composition and flow rate. At the same time, the joint strength can be greatly improved by combining appropriate laser welding process parameters for lap welding of aluminum-silicon coated hot-formed ultra-high-strength steel. The method is simple in process and low in implementation cost. It does not require the removal of the steel surface coating, nor does it require the use of a complex laser welding process with additional processes. It can optimize the weld structure to achieve the purpose of improving the joint strength by only passing a special gas component into the weld and controlling the laser parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0021] like Figure 1 As shown, the present invention provides a simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating, comprising the following steps:
[0022] Step 1: pre-treat the double-sided aluminum-silicon coated hot-formed ultra-high-strength steel plate, overlap the welding parts of the two aluminum-silicon coated hot-formed ultra-high-strength steel plates, and fix them on the welding platform with a welding fixture;
[0023] Step 2: Use a vent pipe to output a specially selected gas that can promote the formation of more austenite structure in the weld to the welding pool; the specially selected gas is a mixed gas composed of Ar and N2;
[0024] Step 3: Start the laser welding system, melt the base material by laser to perform welding, and form a weld after cooling; during the welding process, adjust the ratio and flow of the selected gas, and control the laser process parameters, and adjust the weld structure to reduce the aggregation of the coating in the weld, especially reduce the aggregation of the coating at the fusion line, so as to obtain a higher strength lap joint; wherein, the gas flow rate of the selected gas is 20-30L / min, and the angle between the vent pipe and the weld is 30-60°; wherein, the incident angle of the laser is 85-90°, the power of the laser is 2-4kW, and the welding speed is 1-3m / min.
[0025] In order to improve the cleaning effect and fully ensure the subsequent welding quality, the pretreatment method in step 1 is as follows:
[0026] First, use a cotton ball dipped in an organic solvent to wipe the front and back surfaces of the aluminum-silicon coated hot-formed ultra-high-strength steel plate to remove surface impurities; then quickly blow dry the wiped aluminum-silicon coated hot-formed ultra-high-strength steel plate, and then place it in a dry place for welding.
[0027] Preferably, the organic solvent is acetone.
[0028] In order to strictly control the content of alloy elements to obtain a weld with better tensile strength, in step three, the volume percentage content of N2 in the selected gas is 90% to 40%.
[0029] Preferably, in step one, the thickness of the aluminum-silicon coated hot-formed ultra-high strength steel is 0.5 to 3.5 mm, and the thickness of the aluminum-silicon coating in the aluminum-silicon coated hot-formed ultra-high strength steel is 30 to 70 μm.
[0030] In order to better reduce the degree of aggregation of the coating at the fusion line so as to obtain a lap joint with higher strength, in step three, the volume percentage of N2 in the selected gas is 70%, the gas flow rate is 25L / min, and the angle between the vent pipe and the weld is 45°; in step three, the incident angle of the laser is 85°, the laser power is 3kW, and the welding speed is 1m / min.
[0031] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.
[0032] Embodiment 1:
[0033] This embodiment provides a simple high-quality silicon-coated hot-formed ultra-high-strength steel laser welding method, comprising: welding the aluminum-silicon-coated hot-formed ultra-high-strength steel that has been pre-treated before welding according to Figure 1The lap joint is assembled in the manner shown, and a mixed gas of Ar+70% N2 is introduced into the weld, with a gas flow rate of 25L / min, and the vent pipe forms an angle of 30° with the weld. The incident angle of the laser is 85°, the power of the laser is 2kW, and the welding speed is 1m / min. The weld of this process has been tested by tensile test, and the joint breaks at the fusion line; the tensile strength of the joint can reach 990MPa, which is much higher than the strength of the joint without mixed gas (about 450MPa).
[0034] Embodiment 2:
[0035] This embodiment provides a simple high-quality silicon-coated hot-formed ultra-high-strength steel laser welding method. Figure 1 The lap joint is assembled in the manner shown, and a mixed gas of Ar+40% N2 is introduced into the weld, with a gas flow rate of 20L / min, and the vent pipe forms an angle of 60° with the weld. The incident angle of the laser is 85°, the power of the laser is 4kW, and the welding speed is 3m / min. The weld of this process has been tested by tensile test, and the joint breaks at the fusion line; the tensile strength of the joint can reach 944MPa, which is much higher than the strength of the joint without mixed gas (about 450MPa).
[0036] Comparative Example 1:
[0037] The patent with publication number CN114346439A provides a method for improving the performance of laser lap welding joints of aluminum-silicon coated hot-formed high-strength steel by adding nickel powder, and laps aluminum-silicon coated hot-formed high-strength steel. A layer of pure nickel powder with a particle size of 300 mesh and a thickness of 100μm is spread on the lap plate. The laser welding process is: the laser power is 2.5kW, the welding speed is 1m / min, and when argon is used for protection, the flow rate of argon is 15L / min. The resulting weld is well formed. The joint breaks at the fusion line, and the strength is only 772MPa, which is much lower than the tensile strength in this embodiment.
[0038] Comparative Example 2:
[0039] The patent with publication number CN115026429A is for adding C35%+Fe65% alloy powder to laser overlap aluminum silicon coating hot forming ultra-high strength steel. The alloy powder is bonded and laid on the weld bead with a binder for 150μm. The length of the joint overlap is 10mm, the overlap gap is 0.1mm, the laser incident angle is 85°, the laser power is 4kW, the welding speed is 3m / min, and when argon is used for protection, the argon flow rate is 15L / min. The resulting weld is well formed. The joint breaks at the fusion line, and the strength is only 746MPa, which is also far lower than the tensile strength in this embodiment.
[0040] In the present invention, by pretreatment, impurities such as oil stains on the surface of aluminum-silicon coated hot-formed ultra-high-strength steel can be effectively removed, which is conducive to ensuring the subsequent welding quality. By controlling the laser process and coordinating the protection of special gases, the weld structure can be effectively adjusted, the aggregation degree of the coating in the weld can be reduced, especially the aggregation degree of the coating at the fusion line is reduced, thereby obtaining a higher strength lap joint. After thousands of experiments, it was found that in addition to austenite stabilizing elements such as Ni and C, N is also a strong austenitizing stabilizing element, and the addition method of N can be added without presetting. Its addition method is relatively special. Since a protective gas is introduced into the molten pool during welding, N can be mixed in the protective gas as N2 gas (the commonly used protective gas for laser welding steel is argon). Using Ar+N2 mixed gas to the molten pool, N can enter the weld in a non-contact form. According to the basic theory of materials science and welding metallurgy, the high-temperature molten pool can absorb a large amount of N, and then the amount of N dissolved can be guaranteed. Controlling the amount of N dissolved is mainly solved by changing the proportion of the mixed gas and the gas flow rate. Therefore, the performance of welded joints can be improved simply and effectively through this non-contact method of adding alloying elements.
[0041] The present invention can dissolve the austenitized alloying element N into the weld in a non-contact manner by passing a gas containing N into the weld, which not only simplifies the method of adding alloying elements, but also can conveniently strictly control the content of alloying elements by controlling the gas composition and flow rate. At the same time, the joint strength can be greatly improved by combining appropriate laser welding process parameters for lap welding of aluminum-silicon coated hot-formed ultra-high-strength steel. The method is simple in process and low in implementation cost. It does not require the removal of the steel surface coating, nor does it require the use of a complex laser welding process with additional processes. It can optimize the weld structure to achieve the purpose of improving the joint strength by only passing a special gas component into the weld and controlling the laser parameters.
Claims
1. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating, It is characterized in that The steps include: Step 1: pre-treat the double-sided aluminum-silicon coated hot-formed ultra-high-strength steel plate, overlap the welding parts of the two aluminum-silicon coated hot-formed ultra-high-strength steel plates, and fix them on the welding platform with a welding fixture; Step 2: Use a vent pipe to output a specially selected gas that can promote the formation of more austenite structure in the weld to the welding pool; the specially selected gas is composed of Ar and N 2 The gas mixture is composed of Step 3: Start the laser welding system, use the laser to melt the base material for welding, and form a weld after cooling; During the welding process, the ratio and flow rate of the selected gas are adjusted, and the laser process parameters are controlled. By adjusting the weld structure, the aggregation degree of the coating in the weld is reduced to obtain a higher strength lap joint; wherein, the gas flow rate of the selected gas is 20-30L / min, and the angle between the vent pipe and the weld is 30-60°; wherein, the incident angle of the laser is 85-90°, the laser power is 2-4kW, and the welding speed is 1-3m / min.
2. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating according to claim 1, It is characterized in that, The preprocessing method in step 1 is as follows: First, use a cotton ball dipped in an organic solvent to wipe the front and back surfaces of the aluminum-silicon coated hot-formed ultra-high-strength steel plate to remove surface impurities; then quickly blow dry the wiped aluminum-silicon coated hot-formed ultra-high-strength steel plate, and then place it in a dry place for welding.
3. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating according to claim 2, It is characterized in that The organic solvent is acetone.
4. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating according to any one of claims 1 to 3, It is characterized in that In step 3, N in the selected gas 2 The volume percentage content is 90% to 40%.
5. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating according to any one of claims 1 to 3, It is characterized in that In step one, the thickness of the aluminum-silicon coated hot-formed ultra-high strength steel is 0.5 to 3.5 mm, and the thickness of the aluminum-silicon coating in the aluminum-silicon coated hot-formed ultra-high strength steel is 30 to 70 μm.
6. A simple and high-quality laser welding method for hot-formed ultra-high-strength steel with aluminum-silicon coating according to claim 4, It is characterized in that In step 3, N in the selected gas 2 The volume percentage content is 70%, the gas flow rate is 25L / min, and the angle between the vent pipe and the weld is 45°; in step three, the incident angle of the laser is 85°, the laser power is 3kW, and the welding speed is 1m / min.
Citation Information
Patent Citations
Method for improving performance of aluminum-silicon coating hot-formed ultrahigh-strength steel laser welding head
CN114346439A
Welding method for improving performance of aluminum-silicon coating hot-formed ultrahigh-strength steel joint for automobile
CN115026429A
Manufacturing method of aluminum-silicon coated steel / high-strength hot-formed steel composite steel part
CN111843214A
Split type high-order laser beam based tailor welding method for automotive aluminum-silicon coated steel plates
CN113560720A
Tailored blank laser welding method for aluminum-silicon coating hot forming steel
CN116441708A