Manufacturing method of scrimber

Through the recombinant wood production method without dissolution, using cutting, drying, balance and curing steps, combined with alkaline phenolic glue, the damage and deformation problems caused by dissolution of wood in the prior art are solved, and the production efficiency and physics are improved Mechanical properties and make the wood grain more beautiful.

CN118977299AInactive Publication Date: 2024-11-19JIANGSU HANZHIYUAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310523546.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing recombinant wood needs to be dissociated during the production process, resulting in damage and texture deformation of the wood, which is costly and inefficient in production, and cannot avoid waste of materials.

Method used

Recombinant wood is made by cutting, pre-glue drying, pre-glue balance, immersion, post-glue balance, post-glue drying, post-glue balance, post-glue drying, post-glue balance, blanking, pressing and curing, etc. Alkaline phenolic glue is used as a cementitious agent, and the temperature and duration of each process are adjusted to improve product performance.

Benefits of technology

The production of recombinant wood without detachment is achieved, which improves work efficiency and reduces material waste. The physical and mechanical properties of the product are better, and warping, deformation and cracking problems are reduced, making the wood grain more beautiful.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977299A_ABST
    Figure CN118977299A_ABST
Patent Text Reader

Abstract

According to the manufacturing method of the scrimber, raw wood or waste veneers are used as raw materials, and the manufacturing method comprises the steps of cutting, drying before gluing, gum dipping, drying after gluing, assembling, pressing and curing, specifically, the pressed plate is heated and cured. And balancing is carried out before impregnation, after impregnation, after drying and after curing. The method has the advantages that wood does not need to be defibered, and waste of raw materials is reduced; 2, gum dipping is more uniform in the gum dipping process; 3, parameters such as temperature and duration of each process are reasonably arranged for wood, and a series of problems such as product warping, deformation and cracks are reduced; and 4, the wood grains are more attractive than the traditional scrimber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wood processing, in particular to a method for preparing a novel reconstituted wood. Background Art

[0002] Existing reconstituted wood is made by decomposing wood into "wood bundles" and re-modifying and combining them without disrupting the arrangement direction of wood fibers and retaining the basic characteristics of wood, to make a new type of wood with high strength and large specifications to replace solid hardwood, and its performance is better than solid hardwood. However, decomposing wood into "wood bundles" or "wood bundle curtains" requires special decomposition equipment, and the decomposition process will not only cause damage to the wood, but also cause deformation of the wood texture.

[0003] If the production of reconstituted wood can be carried out without deflashing, it can save costs, significantly improve production efficiency and reduce material waste. Summary of the invention

[0004] The purpose of the present invention is to improve the deficiencies of the prior art and provide a reconstituted wood having better physical and mechanical properties than the raw wood constituting the reconstituted wood.

[0005] The technical solution adopted by the present invention to solve the above technical problems is: A method for manufacturing reconstituted wood, wherein the raw material used is logs or waste veneers, comprising the following steps: Cutting: Peeling and cutting logs into boards of a certain width; or cutting waste veneers into boards of a certain width; the thickness of the boards is 0.5mm-2.8mm; the boards are not thinned; Drying before gluing: Dry the wood board before gluing to reduce the moisture content of the wood board; Balance before gluing: balance the internal structure of the wood board after drying before gluing; Dipping: Dipping the wood board into a dipping tank filled with adhesive so that the wood board bundle is fully covered with adhesive; Balance after gluing: balance the wood board after gluing, so that the adhesive can fully and evenly penetrate into the wood board; Drying after gluing: Put the glue-impregnated wood board into the drying equipment for drying, and reduce the moisture content of the wood board to 8%-20%; Balance after drying: balance the internal structure of the wood board after gluing and drying; Assembly and pressing: The balanced wood boards are assembled and placed in the pressing equipment to be pressed into boards; Curing: Heat and cure the pressed sheet.

[0006] As a further improvement, the drying before gluing is carried out at a temperature of 80°C-130°C, so that the moisture content of the eucalyptus wood formwork is reduced to 0-12%; As a further improvement, the binder is alkaline phenolic glue.

[0007] As a further improvement, the dipping time is 15 minutes to 30 minutes.

[0008] As a further improvement, the binder in the dipping tank is fluid.

[0009] As a further improvement, the temperature of post-gluing drying is between 50°C and 70°C.

[0010] As a further improvement, the pre-gel balancing time is at least 3 hours.

[0011] As a further improvement, the balancing time after gluing is at least 6 hours; if the raw wood species is ginkgo, the balancing time after gluing is at least 12 hours.

[0012] As a further improvement, the balancing time after drying is at least 12 hours; if the raw wood species is ginkgo, the balancing time after gluing is at least 24 hours.

[0013] As a further improvement, after curing, the product is subjected to post-curing balancing, and the post-curing balancing time is at least 7 days.

[0014] The advantages of the present invention are: 1. There is no need to thin the wood, which improves work efficiency; 2. The gluing process is more uniform; 3. The temperature and duration of each process are reasonably arranged according to the wood, reducing a series of problems such as product warping, deformation, and cracks; 4. The wood grain is more beautiful than traditional reconstituted wood. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a flow chart of the method for producing reconstituted wood of the present invention. DETAILED DESCRIPTION

[0016] The embodiments of the present invention are further described below in conjunction with the accompanying drawings. Example

[0017] A method for manufacturing reconstituted wood, wherein the raw material used is eucalyptus logs, comprising the following steps: Cutting: The eucalyptus logs are peeled and cut into boards with a width of 150 mm and a thickness of 1.4 mm. The boards are not thinned. Since the wood is not thinned, the boards need to be cut thinner than the existing technology. This also avoids a large amount of raw material waste during the thinning process.

[0018] Drying before gluing: Dry the wood board before gluing to reduce the moisture content of the wood board. The temperature is 80℃-130℃, so that the moisture content of the eucalyptus wood board can be reduced to 0-12%; Balance before gluing: Balance the internal structure of the board after drying before gluing. The balancing time is 4 hours. Compared with the existing technology, this process is added to make the internal structure of the board tend to be stable.

[0019] Dipping: Dipping the wood board into a dipping tank filled with alkaline phenolic glue, so that the wood board bundle is fully covered with adhesive. During the dipping process, the alkaline phenolic glue is allowed to flow fully. The dipping time is 15 to 30 minutes.

[0020] Balance after gluing: Balance the wood board after gluing, so that the adhesive can fully and evenly penetrate into the wood board. The balance time after gluing is 8 hours, which is longer than the existing technology.

[0021] Drying after gluing: Put the glue-impregnated wood board into the drying equipment for drying, and reduce the moisture content of the wood board to 8%-20%. The drying temperature after gluing is 50℃-70℃; Balance after drying: Balance the internal structure of the wood board after gluing and drying. The balancing time is 15 hours, which is longer than the balancing time after drying in the prior art.

[0022] Assembly and pressing: The balanced wood boards are assembled and placed in the pressing equipment to be pressed into boards; Curing: The pressed board is heated and cured, and the balancing time after curing is 7 days. Example

[0023] A method for manufacturing reconstituted wood, wherein the raw material used is ginkgo logs, comprising the following steps: Cutting: The ginkgo logs are peeled and cut into wooden boards with a width of 160mm and a thickness of 1.3mm. The wooden boards are not thinned.

[0024] Drying before gluing: Dry the wood board before gluing to reduce the moisture content of the wood board. The temperature is 80℃-130℃, so that the moisture content of the ginkgo wood board can be reduced to 0-12%; Balance before gluing: Balance the internal structure of the wooden board after drying before gluing. The balancing time is 4 hours.

[0025] Dipping: Dip the wood board into a dipping tank filled with alkaline phenolic glue, so that the wood board bundle is fully coated with adhesive, and the alkaline phenolic glue is fully flowed during the dipping process. The dipping time is 30 minutes. Due to the material of ginkgo wood, a longer dipping time is required.

[0026] Balance after gluing: Balance the wood board after gluing, so that the adhesive can fully and evenly penetrate into the wood board. The balance time after gluing is 24 hours. Due to the material of ginkgo wood, a longer balance time is required. Drying after gluing: Put the glue-impregnated wood board into the drying equipment for drying, and reduce the moisture content of the wood board to 8%-20%. The drying temperature after gluing is 50℃-70℃; Balance after drying: Balance the internal structure of the board after gluing and drying. The balancing time is 36 hours. Due to the material of ginkgo wood, a longer balancing time after drying is required; Assembly and pressing: The balanced wood boards are assembled and placed in the pressing equipment to be pressed into boards; Curing: The pressed board is heated and cured, and the balancing time after curing is 14 days.

[0027] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the present invention, or are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for manufacturing reconstituted wood, characterized in that: The raw materials used are logs or waste veneers, and the process includes the following steps: a. Cutting: Peel and cut logs into boards of a certain width; or cut waste veneers into boards of a certain width; the thickness of the boards is 0.5mm-2.8mm; No debonding of the planks; b. Drying before gluing: Dry the wood before gluing to reduce the moisture content of the wood; c. Balance before gluing: balance the internal structure of the board after drying before gluing; d. Dipping: Dipping the wood board into a dipping tank filled with adhesive so that the wood board bundle is fully covered with adhesive; e. Balance after gluing: Balance the wood board after gluing, so that the adhesive can fully and evenly penetrate into the wood board; f. Drying after gluing: Put the glue-impregnated wood board into the drying equipment for drying, and reduce the moisture content of the wood board to 8%-20%; g. Balance after drying: balance the internal structure of the wood board after gluing and drying; h. Assembly and pressing: Assemble the balanced wood boards after gluing and place them in a pressing device to press them into boards; i. Curing: Heat and cure the pressed sheet.

2. The method for producing reconstituted wood according to claim 1, characterized in that: The drying before gluing is carried out at a temperature of 80°C-130°C, so that the moisture content of the eucalyptus wood formwork is reduced to 0-12%.

3. The method for producing reconstituted wood according to claim 1, characterized in that: The binder is alkaline phenolic glue.

4. The method for producing reconstituted wood according to claim 1, characterized in that: The dipping time is 15 to 30 minutes.

5. The method for producing reconstituted wood according to claim 1, characterized in that: The binder in the dipping tank is fluid.

6. The method for producing reconstituted wood according to claim 1, characterized in that: The drying temperature after gluing is 50℃-70℃.

7. The method for producing reconstituted wood according to claim 1, characterized in that: The pre-gel balancing time is at least 3 hours.

8. The method for producing reconstituted wood according to claim 1, characterized in that: The post-gluing balancing time is at least 6 hours; if the raw wood species is ginkgo, the post-gluing balancing time is at least 12 hours.

9. The method for producing reconstituted wood according to claim 1, characterized in that: The balancing time after drying is at least 12 hours; if the raw wood species is ginkgo, the balancing time after gluing is at least 24 hours.

10. The method for producing reconstituted wood according to claim 1, characterized in that: After curing, the product is subjected to post-curing equilibration, and the post-curing equilibration time is at least 7 days.