Preparation method of composite steel-concrete composite beam
Patent Information
- Application Number
- CN202411062603.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
Abstract
Description
Technical Field
[0001] The invention relates to the field of bridges, and in particular to a method for preparing a composite steel-concrete composite beam. Background Art
[0002] The steel-concrete composite beam is a new type of structure developed on the basis of steel structure and concrete structure. It mainly resists the lifting and relative sliding of the two at the interface by setting shear connectors (studs, channel steel, bending bars, etc.) between the steel beam and the concrete flange plate, so that they can work together as a whole. The steel-concrete composite beam has excellent properties such as strong bearing capacity, light weight, less materials, good seismic performance and short construction period, which makes the steel-concrete composite structure show its broad application prospects in high-rise and super-high-rise buildings, large-span bridges, underground projects, mining projects, port projects, and combined reinforcement and repair projects.
[0003] However, the steel-concrete composite beams that are widely used in actual projects also have some problems in their application. Ordinary concrete bridge decks have heavy weight and low strength, and the joint structure is complex and easy to seep water, and the durability is poor. As a result, when used as a bridge, the structural strength is insufficient, the risk of structural failure increases, and the advantages of the composite bridge cannot be fully utilized. Ultra-high performance concrete (Ultra-high Performance Concrete, UHPC) materials have ultra-high strength and excellent durability due to the high density of the matrix. The use of UHPC materials to replace ordinary concrete to form prefabricated steel-UHPC composite beam bridges is expected to overcome the above technical difficulties. However, the current strength of ultra-high performance concrete still cannot meet the demand, and cracking and water seepage often occur during the application process. Summary of the invention
[0004] In view of the problems existing in the prior art, an object of the present invention is to provide a method for preparing a composite steel-concrete composite beam.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] A method for preparing a composite steel-concrete composite beam comprises the following steps:
[0007] Step 1, select appropriate steel sections and cut them according to the designed size, and then grind, remove rust and coat them to obtain prefabricated steel sections;
[0008] Step 2, welding the steel bars to the appropriate positions of the prefabricated steel sections, cleaning the surface of the welded steel sections, and obtaining the steel sections after welding the steel bars;
[0009] Step 3, mixing according to the ingredient formula of ultra-high performance concrete, and stirring evenly to obtain an ultra-high performance concrete mixture;
[0010] Step 4, embedding the steel section after welding the steel bars in the mold, and then pouring the ultra-high performance concrete mixture into the mold. After curing, the mold is removed to obtain a prefabricated steel section-concrete plate;
[0011] Step 5, punching the prefabricated steel-concrete plate according to the design drawing, leaving the required holes, and then grinding to obtain a prefabricated steel-concrete composite plate with holes;
[0012] Step 6: transport the prefabricated steel-concrete panels with holes to the construction site, assemble them according to the design drawings, and position and fix them so that the panels meet the required design requirements and remain stable;
[0013] Step 7, after the plate is fixed, the corresponding gaps and holes are poured and cured again using ultra-high performance concrete mixture, thus completing the preparation of the composite steel-concrete composite beam.
[0014] Preferably, the ingredients of the ultra-high performance concrete, calculated by weight, include:
[0015] 80-120 parts of cement, 118-174 parts of coarse aggregate, 92-110 parts of fine aggregate, 30-50 parts of fly ash, 15-35 parts of modified sepiolite fiber, 0.8-1.6 parts of water reducer and 42-84 parts of water.
[0016] Preferably, the cement is ordinary Portland cement PO42.5; the coarse aggregate is crushed stone with a particle size of 5-10 mm; and the fine aggregate is river sand with a particle size of 0.075-4.75 mm.
[0017] Preferably, the silicon powder is first-grade fly ash, and the fineness requirement is that the residue on a 45 μm square hole sieve is no more than 12%.
[0018] Preferably, the water reducer is polycarboxylate water reducer ZY-1010.
[0019] Preferably, the preparation method of the modified sepiolite fiber comprises:
[0020] S1. Place the sepiolite fiber in a Tris-HCl buffer solution, disperse it evenly by ultrasonication, then add dopamine hydrochloride, stir and treat it at room temperature for 24-48 hours, then filter out the fiber, wash it three times with water, and dry it in an oven to obtain dopamine-modified sepiolite fiber;
[0021] S2, adding eugenol to epibromopropane, stirring evenly under the protection of nitrogen, then adding tetrabutylammonium bromide, heating to 110-120°C, stirring at this temperature for 2-4 hours, then cooling to 60-70°C, adding sodium hydroxide solution dropwise, stirring at this temperature for 2-4 hours, to obtain epoxidized eugenol;
[0022] S3. Dissolve epoxidized eugenol in toluene, then add dopamine-modified sepiolite fiber, mix thoroughly, heat to 60-80°C, keep warm and stir for 5-15h, after treatment, remove the solvent under reduced pressure, and obtain modified sepiolite fiber after drying.
[0023] Preferably, in S1, the concentration of Tris-HCl buffer is 0.05-0.1 mol / L; the diameter of the sepiolite fiber is 10 μm and the length is 5 cm.
[0024] Preferably, in S1, the mass ratio of sepiolite fiber, dopamine hydrochloride and Tris-HCl buffer is 1:0.1-0.2:20-40.
[0025] Preferably, in S2, the mass ratio of eugenol, tetrabutylammonium bromide and epibromopropane is 1.6-3.2:0.02-0.07:1.4-2.8.
[0026] Preferably, in S2, the mass fraction of the sodium hydroxide solution is 10%-20%; the mass ratio of eugenol to the sodium hydroxide solution is 1:1.1-1.5.
[0027] Preferably, in S3, the mass ratio of dopamine-modified sepiolite fiber, epoxidized eugenol and toluene is 1:0.5-1:20-30.
[0028] The beneficial effects of the present invention are:
[0029] 1. The present invention prepares a method for preparing a composite steel-concrete composite beam. The concrete material used in the preparation process is ultra-high performance concrete, which has more excellent performance than conventional concrete materials, so that the composite steel-concrete composite beam prepared by the present invention has the advantages of being lighter, higher in strength, more resistant to cracking and more resistant to water seepage.
[0030] 2. The ultra-high performance concrete prepared by the present invention is based on cement material, and modified sepiolite fiber is added as a modified additive to replace part of the gravel. It is not only lighter, but also enhances the strength of the concrete material. In addition, it has been found through testing that it also has good performance in crack resistance and water seepage resistance.
[0031] 3. The modified sepiolite fiber is prepared by combining dopamine-modified sepiolite fiber with epoxidized eugenol. The prepared modified sepiolite fiber not only has good dispersibility in concrete, but also has a certain enhancement effect on the performance of concrete. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0033] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0034] The present invention will be further described below in conjunction with the following examples.
[0035] Example 1
[0036] A method for preparing a composite steel-concrete composite beam comprises the following steps:
[0037] Step 1, select appropriate steel sections and cut them according to the designed size, and then grind, remove rust and coat them to obtain prefabricated steel sections;
[0038] Step 2, welding the steel bars to the appropriate positions of the prefabricated steel sections, cleaning the surface of the welded steel sections, and obtaining the steel sections after welding the steel bars;
[0039] Step 3, mixing according to the ingredient formula of ultra-high performance concrete, and stirring evenly to obtain an ultra-high performance concrete mixture;
[0040] Step 4, embedding the steel section after welding the steel bars in the mold, and then pouring the ultra-high performance concrete mixture into the mold. After curing, the mold is removed to obtain a prefabricated steel section-concrete plate;
[0041] Step 5, punching the prefabricated steel-concrete plate according to the design drawing, leaving the required holes, and then grinding to obtain a prefabricated steel-concrete composite plate with holes;
[0042] Step 6: transport the prefabricated steel-concrete panels with holes to the construction site, assemble them according to the design drawings, and position and fix them so that the panels meet the required design requirements and remain stable;
[0043] Step 7, after the plate is fixed, the corresponding gaps and holes are poured and cured again using ultra-high performance concrete mixture, thus completing the preparation of the composite steel-concrete composite beam.
[0044] In the above, the ingredients of ultra-high performance concrete are calculated by weight and include:
[0045] 100 parts of cement, 136 parts of coarse aggregate, 103 parts of fine aggregate, 40 parts of fly ash, 25 parts of modified sepiolite fiber, 1.2 parts of water reducer and 63 parts of water.
[0046] Among them, cement is ordinary Portland cement PO42.5; coarse aggregate is crushed stone with a particle size of 5-10mm; fine aggregate is river sand with a particle size of 0.075-4.75mm; silica powder is first-class fly ash, and the fineness requirement is that the residue on the 45μm square hole sieve is not more than 12%; the water reducer is polycarboxylic acid water reducer ZY-1010.
[0047] Wherein, the preparation method of modified sepiolite fiber comprises:
[0048] S1. Place sepiolite fiber with a diameter of 10 μm and a length of 5 cm in a 0.05-0.1 mol / L Tris-HCl buffer, disperse it evenly by ultrasonication, then add dopamine hydrochloride, the mass ratio of sepiolite fiber, dopamine hydrochloride and Tris-HCl buffer is 1:0.15:30, stir at room temperature for 36 hours, filter out the fiber, wash it three times with water, and dry it in an oven to obtain dopamine-modified sepiolite fiber;
[0049] S2, add eugenol to epibromopropane, stir well under the protection of nitrogen, then add phase transfer catalyst tetrabutylammonium bromide, the mass ratio of eugenol, tetrabutylammonium bromide and epibromopropane is 2.4:0.05:2.1, heat to 110°C, keep warm and stir for 3h, then cool to 65°C, add dropwise 15% sodium hydroxide solution, the mass ratio of eugenol to sodium hydroxide solution is 1:1.2, keep warm and stir for 3h, and obtain epoxidized eugenol;
[0050] S3. Dissolve epoxidized eugenol in toluene, then add dopamine-modified sepiolite fiber, the mass ratio of dopamine-modified sepiolite fiber, epoxidized eugenol and toluene is 1:0.6:25. After fully mixing, heat to 70°C, keep stirring for 10 hours, and after the treatment, remove the solvent under reduced pressure. After drying, obtain modified sepiolite fiber.
[0051] Example 2
[0052] A method for preparing a composite steel-concrete composite beam is different from that of Example 1 in that the composition of the ultra-high performance concrete is different.
[0053] The ingredients of ultra-high performance concrete, calculated by weight, include:
[0054] 80 parts of cement, 118 parts of coarse aggregate, 92 parts of fine aggregate, 30 parts of fly ash, 15 parts of modified sepiolite fiber, 0.8 parts of water reducer and 42 parts of water.
[0055] Among them, cement is ordinary Portland cement PO42.5; coarse aggregate is crushed stone with a particle size of 5-10mm; fine aggregate is river sand with a particle size of 0.075-4.75mm; silica powder is first-class fly ash, and the fineness requirement is that the residue on the 45μm square hole sieve is not more than 12%; the water reducer is polycarboxylic acid water reducer ZY-1010.
[0056] Wherein, the preparation method of modified sepiolite fiber comprises:
[0057] S1. Place sepiolite fiber with a diameter of 10 μm and a length of 5 cm in a 0.05 mol / L Tris-HCl buffer, disperse it evenly by ultrasonication, then add dopamine hydrochloride, the mass ratio of sepiolite fiber, dopamine hydrochloride and Tris-HCl buffer is 1:0.1:20, stir at room temperature for 24 hours, filter out the fiber, wash it three times with water, and dry it in an oven to obtain dopamine-modified sepiolite fiber;
[0058] S2, add eugenol to epibromopropane, stir well under the protection of nitrogen, then add phase transfer catalyst tetrabutylammonium bromide, the mass ratio of eugenol, tetrabutylammonium bromide and epibromopropane is 1.6:0.02:1.4, heat to 110°C, keep warm and stir for 2h, then cool to 60°C, add dropwise 10% sodium hydroxide solution, the mass ratio of eugenol to sodium hydroxide solution is 1:1.1, keep warm and stir for 2h, and obtain epoxidized eugenol;
[0059] S3. Dissolve epoxidized eugenol in toluene, then add dopamine-modified sepiolite fiber, the mass ratio of dopamine-modified sepiolite fiber, epoxidized eugenol and toluene is 1:0.5:20. After fully mixing, heat to 60°C, keep stirring for 5 hours, and after the treatment, remove the solvent under reduced pressure. After drying, the modified sepiolite fiber is obtained.
[0060] Example 3
[0061] A method for preparing a composite steel-concrete composite beam is different from that of Example 1 in that the composition of the ultra-high performance concrete is different.
[0062] The ingredients of ultra-high performance concrete, calculated by weight, include:
[0063] 120 parts of cement, 174 parts of coarse aggregate, 110 parts of fine aggregate, 50 parts of fly ash, 35 parts of modified sepiolite fiber, 1.6 parts of water reducer and 84 parts of water.
[0064] Among them, cement is ordinary Portland cement PO42.5; coarse aggregate is crushed stone with a particle size of 5-10mm; fine aggregate is river sand with a particle size of 0.075-4.75mm; silica powder is first-class fly ash, and the fineness requirement is that the residue on the 45μm square hole sieve is not more than 12%; the water reducer is polycarboxylic acid water reducer ZY-1010.
[0065] Wherein, the preparation method of modified sepiolite fiber comprises:
[0066] S1. Place sepiolite fiber with a diameter of 10 μm and a length of 5 cm in a .1 mol / L Tris-HCl buffer, disperse it evenly by ultrasonication, then add dopamine hydrochloride, the mass ratio of sepiolite fiber, dopamine hydrochloride and Tris-HCl buffer is 1:0.2:40, stir at room temperature for 48 hours, filter out the fiber, wash it three times with water, and dry it in an oven to obtain dopamine-modified sepiolite fiber;
[0067] S2, add eugenol to epibromopropane, stir well under the protection of nitrogen, then add phase transfer catalyst tetrabutylammonium bromide, the mass ratio of eugenol, tetrabutylammonium bromide and epibromopropane is 3.2:0.07:2.8, heat to 120°C, keep warm and stir for 4h, then cool to 70°C, add dropwise 20% sodium hydroxide solution, the mass ratio of eugenol to sodium hydroxide solution is 1:1.5, keep warm and stir for 4h, and obtain epoxidized eugenol;
[0068] S3. Dissolve epoxidized eugenol in toluene, then add dopamine-modified sepiolite fiber, the mass ratio of dopamine-modified sepiolite fiber, epoxidized eugenol and toluene is 1:1:30. After fully mixing, heat to 80°C, keep stirring for 5-15 hours, after treatment, remove the solvent under reduced pressure, and obtain modified sepiolite fiber after drying.
[0069] Comparative Example 1
[0070] An ultra-high performance concrete, which differs from Example 1 only in that the modified sepiolite fiber is replaced by sepiolite fiber.
[0071] Ingredients are calculated by weight and include:
[0072] 100 parts of cement, 136 parts of coarse aggregate, 103 parts of fine aggregate, 40 parts of fly ash, 25 parts of sepiolite fiber, 1.2 parts of water reducer and 63 parts of water.
[0073] Comparative Example 2
[0074] An ultra-high performance concrete, which is different from Example 1 only in that the modified sepiolite fiber is replaced by dopamine-modified sepiolite fiber.
[0075] Ingredients are calculated by weight and include:
[0076] 100 parts of cement, 136 parts of coarse aggregate, 103 parts of fine aggregate, 40 parts of fly ash, 25 parts of dopamine-modified sepiolite fiber, 1.2 parts of water reducer and 63 parts of water.
[0077] The performance of the ultra-high performance concrete of Example 1, Comparative Example 1 and Comparative Example 2 was tested, and the results are shown in the following table:
[0078] 28d compressive strength Splitting tensile strength (MPa) Impermeability grade Example 1 124.1 3.97 P11 Comparative Example 1 103.7 2.18 P8 Comparative Example 2 111.2 2.71 P10
[0079] Therefore, it can be seen that the ultra-high performance concrete prepared in Example 1 not only has high strength, but also has better crack resistance and impermeability.
[0080] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0081] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a composite steel-concrete composite beam, characterized in that: The following steps are involved: Step 1, select appropriate steel sections and cut them according to the designed size, and then grind, remove rust and coat them to obtain prefabricated steel sections; Step 2, welding the steel bars to the appropriate positions of the prefabricated steel sections, cleaning the surface of the welded steel sections, and obtaining the steel sections after welding the steel bars; Step 3, mixing according to the ingredient formula of ultra-high performance concrete, and stirring evenly to obtain an ultra-high performance concrete mixture; Step 4, embedding the steel section after welding the steel bars in the mold, and then pouring the ultra-high performance concrete mixture into the mold. After curing, the mold is removed to obtain a prefabricated steel section-concrete plate; Step 5, punching the prefabricated steel-concrete plate according to the design drawing, leaving the required holes, and then grinding to obtain a prefabricated steel-concrete composite plate with holes; Step 6: transport the prefabricated steel-concrete panels with holes to the construction site, assemble them according to the design drawings, and position and fix them so that the panels meet the required design requirements and remain stable; Step 7, after the plate is fixed, the corresponding gaps and holes are poured and cured again using ultra-high performance concrete mixture, thus completing the preparation of the composite steel-concrete composite beam.
2. The method for preparing a composite steel-concrete composite beam according to claim 1, characterized in that: The components of the ultra-high performance concrete are calculated by weight and include: 80-120 parts of cement, 118-174 parts of coarse aggregate, 92-110 parts of fine aggregate, 30-50 parts of fly ash, 15-35 parts of modified sepiolite fiber, 0.8-1.6 parts of water reducer and 42-84 parts of water.
3. The method for preparing a composite steel-concrete composite beam according to claim 2, characterized in that: The cement is ordinary Portland cement PO42.5; the coarse aggregate is crushed stone with a particle size of 5-10 mm; and the fine aggregate is river sand with a particle size of 0.075-4.75 mm.
4. The method for preparing a composite steel-concrete composite beam according to claim 2, characterized in that: The silicon micropowder is first-grade fly ash, and the fineness requirement is that the residue on a 45 μm square sieve is no more than 12%; the water reducer is polycarboxylate water reducer ZY-1010.
5. The method for preparing a composite steel-concrete composite beam according to claim 2, characterized in that: The preparation method of the modified sepiolite fiber comprises: S1. Place the sepiolite fiber in a Tris-HCl buffer solution, disperse it evenly by ultrasonication, then add dopamine hydrochloride, stir and treat it at room temperature for 24-48 hours, then filter out the fiber, wash it three times with water, and dry it in an oven to obtain dopamine-modified sepiolite fiber; S2, adding eugenol to epibromopropane, stirring evenly under the protection of nitrogen, then adding tetrabutylammonium bromide, heating to 110-120°C, stirring at this temperature for 2-4 hours, then cooling to 60-70°C, adding sodium hydroxide solution dropwise, stirring at this temperature for 2-4 hours, to obtain epoxidized eugenol; S3. Dissolve epoxidized eugenol in toluene, then add dopamine-modified sepiolite fiber, mix thoroughly, heat to 60-80°C, keep warm and stir for 5-15h, after treatment, remove the solvent under reduced pressure, and obtain modified sepiolite fiber after drying.
6. The method for preparing a composite steel-concrete composite beam according to claim 5, characterized in that: In the S1, the concentration of Tris-HCl buffer is 0.05-0.1 mol / L; the diameter of the sepiolite fiber is 10 μm and the length is 5 cm.
7. The method for preparing a composite steel-concrete composite beam according to claim 5, characterized in that: In the S1, the mass ratio of sepiolite fiber, dopamine hydrochloride and Tris-HCl buffer is 1:0.1-0.2:20-40.
8. The method for preparing a composite steel-concrete composite beam according to claim 5, characterized in that: In S2, the mass ratio of eugenol, tetrabutylammonium bromide and epibromopropane is 1.6-3.2:0.02-0.07:1.4-2.
8.
9. The method for preparing a composite steel-concrete composite beam according to claim 5, characterized in that: In S2, the mass fraction of the sodium hydroxide solution is 10%-20%; the mass ratio of eugenol to the sodium hydroxide solution is 1:1.1-1.
5.
10. The method for preparing a composite steel-concrete composite beam according to claim 5, characterized in that: In S3, the mass ratio of dopamine-modified sepiolite fiber, epoxidized eugenol and toluene is 1:0.5-1:20-30.