Mould pressing manufacturing method of composite graphite bipolar plate

By applying field effect and optimizing raw material composition in the molding manufacturing of composite graphite bipolar plates, the problem of insufficient filler fluidity and wetting is solved, the strength and chemical stability of the bipolar plates are improved, and the conductivity uniformity and conductivity are achieved. Its stability meets the needs of mass production and cost reduction.

CN118977434APending Publication Date: 2024-11-19ZHONGKE JIAHONG (FOSHAN) NEW ENERGY TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410920279.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the molding manufacturing of existing composite graphite bipolar plates, there are problems such as insufficient filler fluidity, insufficient temperature and pressure and insufficient polymer filler wetting, resulting in uneven thickness, insufficient strength and air leakage of the bipolar plates, and increasing the polymer content will be This results in a decrease in conductivity and instability in conductivity.

Method used

By applying a field effect, such as an electromagnetic field or force field, during the molding manufacturing process, the arrangement direction of conductive fillers in the polymer matrix is ​​controlled, and the composition and processing procedures of composite graphite bipolar plate raw materials are optimized to ensure that The filler is fully wet and evenly distributed.

Benefits of technology

The high chemical stability and strength improvement of composite graphite bipolar plates are achieved, which avoids the decrease in conductivity and unstable conductivity, and meets the requirements of batch continuous production and cost reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977434A_ABST
    Figure CN118977434A_ABST
Patent Text Reader

Abstract

The invention discloses a mold pressing manufacturing method of a composite graphite bipolar plate, and belongs to the field of fuel cells. The invention discloses a mould pressing manufacturing method of a composite graphite bipolar plate. The mould pressing manufacturing method comprises the following steps: S1, introducing a mixture containing a composite graphite bipolar plate raw material into a prefabricated mould; and S2, applying a field effect on the upper and lower molded plates. According to the method, the traditional machining step is omitted, and cost reduction and batch continuous production of products are achieved; the strength and the high chemical stability of the composite graphite bipolar plate are improved; the ordered control of the arrangement direction of the conductive filler in the polymer matrix is realized, and the reduction of the conductivity in the normal direction relative to the horizontal direction caused by the natural arrangement of the conductive filler is overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a molding manufacturing method for a composite graphite bipolar plate, and belongs to the field of fuel cells. Background Art

[0002] Due to the huge energy consumption in today's society, the environmental problems caused by traditional energy utilization models are becoming increasingly serious. Fuel cells, as chemical devices that directly convert fuel chemical energy into electrical energy, are green and efficient, and are expected to play an important role in the process of national energy transformation. Among many fuel cell systems, high-temperature methanol fuel cells (HTMFCs) have the advantages of strong resistance to impurity poisoning and simple water and heat management. They have broad application prospects in portable power supplies, vehicle power supplies, fixed power stations, and combined heat and power systems. However, the high operating temperature also puts forward higher reliability requirements for each component of HTMFC.

[0003] Bipolar plate is one of the key components of HTMFC, which largely determines the size, weight and thermoelectric performance of the stack. Generally speaking, there are two major types of bipolar plate technology, one based on metal materials and the other based on graphite materials. Metal plates have excellent electrical conductivity, thermal conductivity, processability and mechanical stability. Even at a very small thickness, they are not easy to form cracks or break, and their non-porous structure provides good air tightness. However, the poor chemical stability of metal plates makes their life extremely low in the high temperature acidic environment of HTMFC. Graphite bipolar plates can be made of pure (expanded) graphite or graphite composite materials containing polymer binders. The former is low in price but has low mechanical strength, air tightness and chemical stability, while the latter generally sacrifices part of its electrical conductivity in exchange for higher mechanical strength, air tightness and chemical stability.

[0004] For traditional composite graphite bipolar plates, binders (such as polyphenylene sulfide) can improve the fluidity of the filler and the strength and toughness of the bipolar plate during the manufacturing process, while filling the gaps between the graphites so that the bipolar plate can effectively block the anode and cathode gases, while the graphite itself provides the conductivity of the bipolar plate.

[0005] In order to save the traditional machining steps, achieve cost reduction and batch continuous production of products, one-step molding is an important technical goal of composite graphite bipolar plate production. However, to achieve one-step molding, the following technical difficulties need to be overcome:

[0006] 1. Under molding conditions, the existing fillers have insufficient fluidity, resulting in uneven thickness of the bipolar plates and making it difficult to assemble the battery stack.

[0007] 2. Insufficient strength of the bipolar plates due to insufficient temperature and pressure.

[0008] 3. Insufficient wetting of polymer fillers and graphite results in inadequate filling of pores between particles, leading to air leakage in the bipolar plate.

[0009] The above problems can be solved by increasing the proportion of polymer in the filler, but increasing the polymer content often brings the following problems:

[0010] 1. The conductivity of the bipolar plate decreases and the internal resistance of the stack increases. Even near the conductive percolation threshold, a slight increase in polymer content can lead to a decrease in conductivity by several or even dozens of times.

[0011] 2. Due to problems with the process and its own structural characteristics, conductive fillers often have anisotropy, resulting in the conductivity of the bipolar plate in the horizontal direction being much higher than that in the plane normal direction, reaching several times or even dozens of times. The anisotropy of conductivity also causes the instability of bipolar plate products and increases the internal resistance loss of fuel cells. Summary of the invention

[0012] According to one aspect of the present application, a molding manufacturing method for a composite graphite bipolar plate is provided, which omits the traditional machining steps, realizes cost reduction and batch continuous production of products, and improves the strength and high chemical stability of the composite graphite bipolar plate; realizes the ordered control of the arrangement direction of the conductive filler in the polymer matrix, and overcomes the decrease in conductivity in the normal direction relative to the horizontal direction caused by the natural arrangement of the conductive filler.

[0013] A molding method for manufacturing a composite graphite bipolar plate comprises the following steps:

[0014] S1. introducing a mixture containing composite graphite bipolar plate raw materials into a prefabricated mold;

[0015] S2. Apply field effect to the upper and lower molded plates.

[0016] Optionally, when applying the field effect in step S2, the composite graphite bipolar plate is under molding.

[0017] Optionally, in step S2, the field effect is selected from one of an electromagnetic field effect and a force field effect.

[0018] Optionally, in the electromagnetic field effect, the electromagnetic field is selected from at least one of a square wave, a sine wave, and a steady electromagnetic field.

[0019] Optionally, the electromagnetic field is provided by upper and lower molded plates.

[0020] Insulation is required between the upper and lower molded plates.

[0021] Optionally, in the force field effect, the force field is applied by controlling the movement frequency and direction of the molding cavity.

[0022] Optionally, the molding cavity is in reciprocating vibration or centrifugal motion.

[0023] Optionally, the frequencies of the square wave and the sine wave are independently selected from 0 Hz to 10000 Hz.

[0024] Optionally, the frequencies of the square wave and the sine wave are independently selected from any value among 0Hz, 1Hz, 5Hz, 10Hz, 15Hz, 20Hz, 50Hz, 100Hz, 200Hz, 500Hz, 1000Hz, 2000Hz, 3000Hz, 4000Hz, 5000Hz, 6000Hz, 7000Hz, 8000Hz, 9000Hz, 10000Hz or any range between two thereof.

[0025] Optionally, the square wave and the sine wave last for 5s to 60s.

[0026] Optionally, durations of the square wave and the sine wave are independently selected from any value among 5s, 10s, 15s, 20s, 25s, 30s, 40s, 50s, 60s, or any range between the two.

[0027] Optionally, the reciprocating vibration frequency is 0 Hz to 10000 Hz;

[0028] The angular velocity of the centrifugal motion is 0 rad to 1000 rad.

[0029] Optionally, the reciprocating vibration frequency is independently selected from any value among 0Hz, 1Hz, 5Hz, 10Hz, 15Hz, 20Hz, 50Hz, 100Hz, 200Hz, 500Hz, 1000Hz, 2000Hz, 3000Hz, 4000Hz, 5000Hz, 6000Hz, 7000Hz, 8000Hz, 9000Hz, 10000Hz or any range value between two thereof.

[0030] Optionally, the angular velocity of the centrifugal motion is independently selected from any value among 0rad, 1rad, 5rad, 10rad, 15rad, 20rad, 50rad, 100rad, 200rad, 300rad, 400rad, 500rad, 600rad, 700rad, 800rad, 900rad, 1000rad or any range value between two thereof.

[0031] Optionally, the reciprocating vibration and the centrifugal motion last for 5s to 60s.

[0032] Optionally, the duration of the reciprocating vibration and the centrifugal motion is independently selected from any value among 5s, 10s, 15s, 20s, 25s, 30s, 40s, 50s, 60s, or any range between two values.

[0033] Optionally, in step S1, the composite graphite bipolar plate raw material includes graphite powder, conductive filler, and polymer.

[0034] Optionally, in step S1, the conductive filler is selected from at least one of a fibrous conductive filler and a two-dimensional sheet conductive filler.

[0035] Optionally, in step S1, the filling amount of the conductive filler is 0.1 wt% to 80 wt%.

[0036] Optionally, in step S1, the filling amount of the conductive filler is independently selected from any value among 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt% or any range value between two of them.

[0037] Optionally, in step S1, the polymer is a thermoplastic resin;

[0038] The polymer filling amount is 10 wt% to 45 wt%.

[0039] The polymer filling amount is independently selected from any value among 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt%, 45wt% or any range value between two thereof.

[0040] Optionally, the fibrous conductive filler is selected from at least one of carbon nanotubes, carbon fibers, and metal fibers.

[0041] Optionally, the fibrous conductive filler is carbon fiber or carbon nanotube.

[0042] Optionally, the two-dimensional flaky conductive filler is selected from at least one of graphene, graphene oxide, and flake graphite.

[0043] Optionally, the thermoplastic resin is selected from at least one of polytetrafluoroethylene, polyphenylene sulfide, polyetheretherketone, polyetherimide and polyimide.

[0044] The thermoplastic resin is polyphenylene sulfide.

[0045] The conductive filler may also be selected from other conductive fillers.

[0046] The other conductive fillers are materials that can be expanded into two-dimensional or one-dimensional linear fillers.

[0047] The other conductive fillers are selected from adamantane and C60 octane.

[0048] Optionally, in step S1, the prefabricated mold is introduced and then pressurized, and the pressurization conditions are as follows:

[0049] The temperature is 250℃~350℃;

[0050] The time is 5s to 60s;

[0051] The pressure is 2MPa~20MPa.

[0052] Optionally, the temperature is independently selected from any value of 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, or any range therebetween.

[0053] Optionally, the time is independently selected from any value among 5s, 10s, 15s, 20s, 25s, 30s, 40s, 50s, 60s, or any range therebetween.

[0054] Optionally, the pressure is independently selected from any value among 2 MPa, 3 MPa, 4 MPa, 5 MPa, 7.5 MPa, 10 MPa, 12.5 MPa, 15 MPa, 17.5 MPa, 20 MPa, or any range therebetween.

[0055] The beneficial effects of this application include:

[0056] The present application provides a molding manufacturing method for a composite graphite bipolar plate, which eliminates the traditional machining steps, thereby achieving cost reduction and batch continuous production of products; improving the strength and high chemical stability of the composite graphite bipolar plate; and achieving ordered control of the arrangement direction of the conductive filler in the polymer matrix, thereby overcoming the decrease in conductivity in the normal direction relative to the horizontal direction caused by the natural arrangement of the conductive filler. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a schematic diagram of the principle of the molded composite bipolar plate of Example 1 of the present application.

[0058] List of parts and reference numerals:

[0059] 1. Graphite plate mixed embryo; 2. Conductive filler; 3. Upper mold plate; 4. Lower mold plate. DETAILED DESCRIPTION

[0060] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0061] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0062] Example 1

[0063] The molded composite graphite bipolar plate includes the following components in percentage by weight: 75% graphite powder, 10% carbon fiber and 15% resin mixture, wherein the particle size of the graphite powder is 20 μm to 100 μm, and the resin mixture includes 97% polyphenylene sulfide and 3% polytetrafluoroethylene.

[0064] S1: placing the dried graphite powder, carbon fiber and the pre-modified resin mixture in a stirring container and mixing them evenly to obtain a composite graphite raw material.

[0065] S2: The composite graphite raw material is introduced into the prefabricated mold and maintained at 300°C and 2.5MPa pressure for 20s.

[0066] S3: Under the conditions of S2, a sinusoidal alternating electromagnetic field with a frequency of 100 Hz is applied to the upper and lower mold plates and maintained for 20 seconds.

[0067] S4: Under the conditions of S3, increase the molding pressure until the mold reaches the molding limit and maintain it for 20 seconds.

[0068] S5: demoulding, taking out the molded product and post-treating it at 200°C for 30 minutes.

[0069] S6: Place in a closed space for natural cooling, with the maximum cooling rate not exceeding 10℃ / min.

[0070] Example 2

[0071] The molded composite graphite bipolar plate comprises the following components in percentage by weight: 75% graphite powder, 15% flake graphite and 10% polyphenylene sulfide resin, wherein the particle size of the graphite powder is 20 μm to 100 μm, and the particle size of the flake graphite is 0.05 mm to 0.25 mm.

[0072] S1: placing the dried graphite powder, flake graphite and pre-modified resin mixture in a stirring container and mixing them evenly to obtain a composite graphite raw material.

[0073] S2: The composite graphite raw material is introduced into the prefabricated mold and maintained at 300°C and 2.5MPa pressure for 10s.

[0074] S3: At 300°C, a sinusoidal pressure change with a frequency of 1 Hz is applied to the upper mold plate. The upper limit of the pressure is the mold limit pressure, and the lower limit of the pressure is 2.5 MPa, which is maintained for 30 seconds.

[0075] S4: At 300°C, stop the reciprocating motion of the molding plate, increase the molding pressure until the mold reaches the molding limit, and maintain for 20 seconds.

[0076] S5: demoulding, taking out the molded product and post-treating it at 200°C for 30 minutes.

[0077] S6: Place in a closed space for natural cooling, with the maximum cooling rate not exceeding 10℃ / min.

[0078] Comparative Example 1

[0079] The steps are the same as those in Example 1, except that the field effect is not applied to the upper and lower templates, and the mold is formed directly.

[0080] The performance tests of Example 1 and Comparative Example 1 of the present patent are shown in Table 1. The samples are cut into 3cm*3cm*0.3mm square pieces, and the body resistance is tested by the four-probe method; the contact resistance is tested by pressing the gold-plated plate at a pressure of 1MPa; the phosphoric acid corrosion resistance test is carried out by sealing and placing the samples under 180°C and 85wt% phosphoric acid immersion for 24 hours, and then cleaning and testing the mass change rate of the samples before and after testing; the bending strength test is carried out by the three-point bending method.

[0081] Table 1 Performance test table of Example 1 and Comparative Example 1

[0082] Test items density Actual body resistance Contact resistance Quality change rate Bending strength unit <![CDATA[g / cm 3 ]]> mΩ / cm <![CDATA[mΩ / cm 2 ]]> % MPa Example 1 2.07 13.62 60.30 -0.017 57.46 Comparative Example 1 2.045 14.838 64.80 0.001 56.889

[0083] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A molding method for manufacturing a composite graphite bipolar plate, characterized in that: The following steps are involved: S1. introducing a mixture containing composite graphite bipolar plate raw materials into a prefabricated mold; S2. Apply field effect to the upper and lower molded plates.

2. The molding manufacturing method according to claim 1, characterized in that: When the field effect is applied in step S2, the composite graphite bipolar plate is under molding.

3. The molding manufacturing method according to claim 1, characterized in that: In step S2, the field effect is selected from one of an electromagnetic field effect and a force field effect.

4. The molding manufacturing method according to claim 3, characterized in that: In the electromagnetic field effect, the electromagnetic field is selected from at least one of a square wave, a sine wave, and a steady electromagnetic field; Preferably, the electromagnetic field is provided by upper and lower molded plates.

5. The molding manufacturing method according to claim 3, characterized in that: In the force field effect, the force field is applied by controlling the movement frequency and direction of the molding cavity; Preferably, the molding cavity is in reciprocating vibration or centrifugal motion.

6. The molding manufacturing method according to claim 4, characterized in that: The frequencies of the square wave and the sine wave are independently selected from 0 Hz to 10000 Hz; Preferably, the square wave and the sine wave last for 5s to 60s.

7. The molding manufacturing method according to claim 5, characterized in that: The reciprocating vibration frequency is 0 Hz to 10000 Hz; The angular velocity of the centrifugal motion is 0 rad to 1000 rad; Preferably, the reciprocating vibration and the centrifugal motion last for 5s to 60s.

8. The molding manufacturing method according to claim 1, characterized in that: In step S1, the composite graphite bipolar plate raw materials include graphite powder, conductive filler, and polymer; Preferably, in step S1, the conductive filler is selected from at least one of a fibrous conductive filler and a two-dimensional sheet conductive filler; Preferably, in step S1, the filling amount of the conductive filler is 0.1wt% to 80wt%; Preferably, in step S1, the polymer is a thermoplastic resin; The polymer filling amount is 10 wt% to 45 wt%.

9. The molding manufacturing method according to claim 8, characterized in that: The fibrous conductive filler is selected from at least one of carbon nanotubes, carbon fibers, and metal fibers; Preferably, the two-dimensional flaky conductive filler is selected from at least one of graphene, graphene oxide, and flake graphite; Preferably, the thermoplastic resin is selected from at least one of polytetrafluoroethylene, polyphenylene sulfide, polyetheretherketone, polyetherimide and polyimide.

10. The molding manufacturing method according to claim 1, characterized in that: In step S1, the prefabricated mold is introduced and then pressurized. The pressurization conditions are as follows: The temperature is 250℃~350℃; The time is 5s to 60s; The pressure is 2MPa~20MPa.

Citation Information

Cited By

  • Composite graphite bipolar plate under action of pulsed electric field and preparation method of composite graphite bipolar plate

    CN121270147A

  • Powder compression molding method of graphite bipolar plate and graphite composite bipolar plate

    CN121572507A

  • Powder molding method of graphite bipolar plate and graphite composite bipolar plate

    CN121572507B

  • Flexible graphite bipolar plate of flow battery and preparation method of flexible graphite bipolar plate

    CN121769137A