Glass fiber reinforced polyurethane spraying cover plate and preparation process thereof
By using glass fiber reinforced polyurethane spray cover on the car spare tire cover, combining glass fiber and porous resin layer, the problem of flammability of traditional polyurethane foam is solved, the mechanical strength and flame retardant performance of the cover are improved, and the mechanical strength and flame retardant performance of the cover are enhanced. Car safety.
Patent Information
- Application Number
- CN202411080987.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional polyurethane foam is flammable on the car's spare tire cover, affecting the safety of the car.
A polyurethane spray-coated cover plate with glass fiber reinforced is composed of surface patch, PU layer, glass fiber layer and paper core. A porous resin layer is formed by spraying polyurethane foaming agent, combined with glass fiber reinforcement, to improve mechanical strength and flame retardant performance.
It realizes the improvement of the mechanical strength and flame retardant performance of the cover while reducing the weight of the car, and enhances the safety of the car.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane cover plates, in particular to a glass fiber reinforced polyurethane spray cover plate and a preparation process thereof. Background Art
[0002] In recent years, the automobile industry has developed rapidly and is moving towards lightweight development. Under the premise of ensuring automobile safety, the curb weight of the automobile can be reduced, its power can be effectively improved, and fuel consumption can be reduced. The spare tire cover of the automobile is one of the interior decorations of the trunk of the vehicle, which plays a decorative and load-bearing role. Polyurethane foam is a high molecular polymer formed by the reaction of isocyanate and polyether as the main raw materials. Its components are mixed by equipment, sprayed under high pressure, and foamed on site. It has light weight and compression resistance, and is suitable for use in the structure of automobile covers. However, traditional polyurethane foam is flammable, which is not conducive to the safety of automobiles. Therefore, we propose a glass fiber reinforced polyurethane spray cover and its preparation process. Summary of the invention
[0003] The object of the present invention is to provide a glass fiber reinforced polyurethane spray cover plate and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a glass fiber reinforced polyurethane spray cover plate, which comprises the following structures from top to bottom: a surface patch, a PU layer, a glass fiber layer, a paper core, a glass fiber layer and a PU layer;
[0005] The PU layer is formed by spraying a polyurethane foaming agent, wherein the polyurethane foaming agent component contains phosphorus-containing polyols, and the phosphorus-containing polyols include the following components: 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine, fumaric acid, and hydroxyl-terminated polycarbosilane.
[0006] Furthermore, the paper core is corrugated paper or honeycomb paper with a thickness of 7.5 to 17 mm.
[0007] Furthermore, the weight of the glass fiber layer is 40 to 300 g / m 2 , thickness is 0.07~0.23mm.
[0008] Furthermore, the thickness of the PU layer is 3-8 mm, and the weight is 300-900 g / m 2 .
[0009] Furthermore, the thickness of the surface patch is 0.5-3.0 mm, and the density is 0.07-0.80 g / cm 3 .
[0010] Furthermore, the surface patch is adhered to the surface of the PU layer by polyurethane adhesive.
[0011] A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following processes:
[0012] Take the paper core and stretch it to shape it, and lay glass fiber cloth on its upper and lower surfaces to form two sets of glass fiber layers;
[0013] Spray polyurethane foaming agent on the surface of the upper glass fiber layer; turn over, spray polyurethane foaming agent on the surface of another group of glass fiber layers, mold, foam, and form a PU layer;
[0014] The surface patch is adhered to the surface of the PU layer located above by polyurethane glue to obtain a polyurethane spray cover plate.
[0015] Furthermore, the molding process is as follows: mold temperature 105-115° C., pressure 5-10 MPa, and time 40-50 s.
[0016] Furthermore, the coating temperature of the polyurethane adhesive is 20-40°C, and the adhesive amount is 10-25 g / m 2 .
[0017] In the above technical solution, corrugated paper or honeycomb paper is used as the core material, and glass fibers are arranged on both surfaces thereof, so as to reduce the weight of the structure and increase its strength. Then, with the obtained three-layer structure as the center, polyurethane foaming agent is sprayed on both surfaces, and the porous resin layer helps to reduce the weight of the structure. Hot pressing can fix the lightweight structure and further improve its mechanical strength. Finally, a layer of surface patch is glued on the upper surface of the structure for surface functional decoration, so as to obtain a polyurethane spray cover plate with lightweight and high strength characteristics.
[0018] Further, the polyurethane foaming agent is prepared by the following process:
[0019] The phosphorus-containing polyol, polyether polyol, glass fiber, foaming agent, catalyst and surfactant are mixed, stirred at room temperature for 60 to 90 minutes, heated to 50 to 60° C., and stirred at this temperature for 60 to 120 minutes to obtain component A;
[0020] Isocyanate is used as component B; component A and component B are mixed before use to obtain a polyurethane foaming agent.
[0021] Furthermore, the polyurethane foaming agent includes the following components by mass: 10 to 30 parts of phosphorus-containing polyol, 70 to 90 parts of polyether polyol, 130 to 160 parts of isocyanate, 1 to 2 parts of triethanolamine, 1 to 3 parts of glass fiber, 35 to 40 parts of foaming agent, 1.0 to 1.5 parts of catalyst, and 1 to 2 parts of surfactant.
[0022] Furthermore, the isocyanate is one of polymethylene polyphenyl polyisocyanate (PAPI), diphenylmethane diisocyanate (MDI), and toluene diisocyanate (TDI).
[0023] Further, the isocyanate is polymethylene polyphenyl polyisocyanate (PAPI);
[0024] The catalyst is o-toluenediamine polyether: 401P, which comes from Hebei Yadong Chemical Group Co., Ltd.
[0025] The blowing agent is HFC-365mfc / 227ea, which comes from Solvay in Germany.
[0026] In the above technical solution, the catalyst uses o-toluenediamine polyether, which contains nitrogen atoms and benzene rings in its structure, so that it has autocatalytic activity and good mutual solubility with isocyanate. The prepared polyurethane foam (PU layer) has good dimensional stability and mechanical strength; and can play a flame retardant role to a certain extent. With the increase in the amount of o-toluenediamine polyether, its autocatalytic ability is accelerated, the foam density gradually decreases, the compression strength increases, the flame retardancy increases slightly, the dimensional stability is enhanced, the closed cell rate increases, and the thermal conductivity decreases.
[0027] Furthermore, the spraying of the polyurethane foaming agent adopts a spray foaming agent, and the use environment is: temperature 20-35° C., humidity ≤70%.
[0028] Further, the phosphorus-containing polyol is prepared by the following process:
[0029] Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, the temperature was raised to 75-85° C., melamine was slowly added with stirring within 30 minutes, and the reaction was carried out for 4-5 hours; the mixture was filtered, washed, recrystallized and dried in vacuo to obtain compound A;
[0030] The hydroxy-fumaropimaric acid ester compound is dissolved in acetonitrile; the temperature is raised to 80-90° C., compound A and triethylamine are slowly added within 30 minutes, and the reaction is carried out for 6-7 hours; the precipitate is cooled, washed, and vacuum dried to constant weight to obtain a phosphorus-containing polyol.
[0031] Further, the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide (CAS: 714-87-4), melamine, and triethylamine is (3.5-4.0):1:(3.0-3.5);
[0032] The ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide to anhydrous acetonitrile is (10-15) g / 100 mL.
[0033] Further, the mass ratio of the hydroxy-containing fumaric pimaric acid ester compound, compound A, and triethylamine is (10.8-13.3):1:(0.35-0.50);
[0034] The ratio of the hydroxy-fumaropimaric acid ester compound to acetonitrile is (10 to 15) g / 100 mL.
[0035] In the above technical scheme, the amino group in melamine reacts with the chlorine group in 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide to generate a phosphoramide compound, which is recorded as compound A. Using melamine as the starting component, the rigid group triazine nitrogen heterocycle and phosphorus-containing spirocycle are introduced into the structure of the phosphorus-containing polyol, which can effectively improve its rigidity and heat deformation resistance, increase its initial decomposition temperature, contain nitrogen and phosphorus elements, release nitrogen, ammonia and other gases when heated to dilute the combustible gas, form phosphoric acid, promote the dehydration and carbonization of the material, and phosphoric acid absorbs heat, which can inhibit the oxidation and heating process of CO, and exert gas phase and condensed phase flame retardant effects. At the same time, using melamine as the starting component, the prepared phosphorus-containing polyol has multi-functional and branched properties. Phosphorus-containing polyol is added as a polyol component to a polyurethane foaming agent to participate in the reaction between hydroxyl groups and isocyanate to form a cross-linked network, thereby improving the mechanical strength and flame retardancy of the prepared PU layer and reducing its influence on the heat deformation temperature.
[0036] In the above technical solution, by controlling the amount ratio of melamine and 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, the prepared compound A still contains unreacted chlorine groups, which are reacted with a hydroxyl-containing fumaric acid ester compound to obtain a polyhydroxy compound containing fumaric acid, which is recorded as a phosphorus-containing polyol. Introducing fumaric acid into the structure of the phosphorus-containing polyol can further improve the mechanical strength and thermal stability of the prepared PU layer.
[0037] Further, the hydroxy-containing fumaric acid ester compound is prepared by the following process:
[0038] Mix fumaric acid, hydroxyl-terminated polycarbosilane and a catalyst, and heat to 150-160° C. under nitrogen atmosphere, and stir for 30-60 min; heat to 220-240° C., and react for 4-6 h; and cool to obtain a hydroxyl-containing fumaric acid ester compound.
[0039] Further, the mass ratio of fumaric acid (CAS: 125-66-6) and hydroxyl-terminated polycarbosilane is 10:(8.4-12.5);
[0040] The catalyst is zinc oxide, and the dosage of the zinc oxide is 0.10-0.15% of the total mass of the fumaric acid and the hydroxyl-terminated polycarbosilane.
[0041] Further, the hydroxyl-terminated polycarbosilane is prepared by the following process:
[0042] 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide and pure water are mixed in toluene, heated to 80-85°C, and refluxed for 4-5 hours; alkenyldimethylsilyl chloride is slowly added within 30 minutes, heated to 100°C, and refluxed for 100-150 minutes; cooled, washed with water, and the organic phase is dried, the solvent is removed by rotary evaporation, diluted with toluene, and precipitated with cold methanol to obtain alkenyl-terminated oligosiloxane;
[0043] Under light-proof conditions, alkenyl-terminated oligosiloxane, 2-mercaptoethanol and a photoinitiator are mixed in toluene, stirred and irradiated under ultraviolet light for 20 to 30 minutes, vacuum dried, petroleum ether is added, filtered, rotary evaporated, and vacuum dried to obtain a hydroxyl-terminated polycarbosilane.
[0044] Further, the molar ratio of 1,1-dimethoxysilycyclobutane (CAS: 33446-84-3) and alkenyldimethylchlorosilane is (5-6):1;
[0045] The ratio of 1,1-dimethoxysilycyclobutane, tetramethylammonium hydroxide, pure water and toluene is (5.0~5.2)g:(0.010~0.012)g:50mL:25mL.
[0046] Furthermore, the alkenyldimethylchlorosilane is one of allyldimethylchlorosilane, 5-hexenyldimethylchlorosilane, methacryloylpropyldimethylchlorosilane, 1-alkenylundecanyldimethylchlorosilane and 7-octenyldimethylchlorosilane.
[0047] Further, the mass ratio of alkenyl-terminated oligosiloxane to 2-mercaptoethanol is (11.2-14.6):1;
[0048] The photoinitiator is benzoin dimethyl ether, and the dosage is 1.0-1.5% of the total mass of the alkenyl-terminated oligosiloxane and mercaptoethanol.
[0049] In the above technical scheme, 1,1-dimethoxysilylcyclobutane is hydrolyzed and polymerized, and alkenyl dimethyl chlorosilane is capped to form alkenyl-terminated oligosiloxane; then, by using a click reaction, alkenyl is added to 2-mercaptoethanol under the action of a photoinitiator to obtain a hydroxyl-terminated polycarbosilane. The use of 1,1-dimethoxysilylcyclobutane to introduce Si-C bonds and silylcyclobutane structures into polysiloxane can effectively improve its heat resistance.
[0050] Fumaric acid and hydroxyl-terminated polycarbosilane react to obtain a hydroxyl-containing fumaric acid ester compound. Using zinc oxide as a catalyst, three carboxyl groups in fumaric acid and hydroxyl groups in hydroxyl-terminated polycarbosilane undergo esterification reaction. By controlling the amount of the two reactants, the hydroxyl-containing fumaric acid ester compound has a polyhydroxyl functional group, thereby realizing the preparation of the hydroxyl-containing fumaric acid ester compound. The hydroxyl-containing fumaric acid ester compound with a polyhydroxyl functional group increases the branching degree of the phosphorus-containing polyol, improves the molecular crosslinking degree in the PU layer, and helps to further improve its mechanical strength. In addition, the introduction of polycarbosilane with high heat resistance allows the phosphorus, nitrogen, and silicon in the phosphorus-containing polyol to work together, which can enhance the flame retardancy of the PU layer, capture gas-phase free radicals during combustion, and help to form a denser silicon-rich carbon layer.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1. A glass fiber reinforced polyurethane spray cover plate of the present invention is composed of a surface patch, a PU layer, a glass fiber layer and a paper core. The glass fibers arranged on both sides of the paper core can increase its strength. Then the surface of the obtained three-layer structure is sprayed with a polyurethane foaming agent, and the porous resin layer helps the structure to reduce weight and improve strength. Finally, the surface patch is glued to obtain a polyurethane spray cover plate with lightweight and high strength characteristics.
[0053] 2. A preparation process of a glass fiber reinforced polyurethane spray cover plate of the present invention comprises the following steps: preparing a hydroxyl-terminated polycarbosilane by using 1,1-dimethoxysilycyclobutane, alkenyldimethylchlorosilane and 2-mercaptoethanol, esterifying fumaric acid and the hydroxyl-terminated polycarbosilane to prepare a hydroxyl-containing fumaric acid ester; preparing a phosphorus-containing polyol by using 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine and a hydroxyl-containing fumaric acid ester compound, and using the phosphorus-containing polyol as a polyurethane foaming agent component to effectively improve the mechanical strength and flame retardancy of the prepared PU layer. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] In the following specific implementations, the tests are all small-scale laboratory tests, which can be expanded in equal proportions;
[0056] The paper core is a honeycomb paper core: thickness 10mm, sourced from Foshan Heshenglong Packaging Products Co., Ltd., and the weight after stretching is 300g / m 2 ;
[0057] Glass fiber cloth: weight 200g / m 2 , thickness 0.21mm, from Henan Changyu New Materials Technology Co., Ltd.;
[0058] Surface patch: flame retardant PET felt, density 0.20g / cm 3 , thickness 1.5mm, sourced from Nangong City Jiatong Felt Products Co., Ltd.;
[0059] Polyurethane glue: BEPU5103 A / B, from Shanghai Beco Chemical; the coating temperature of polyurethane glue is 25℃, and the glue amount is 15g / m 2 ;
[0060] Polyether polyol: a mixture of CHE-2801, CHE-303, and CHK-350D in a mass ratio of 3:10:1, sourced from Changhua Chemical Technology Co., Ltd.
[0061] Isocyanate: polymethylene polyphenyl isocyanate PM-200, from BASF AG;
[0062] Glass fiber: Glass fiber powder, particle size 200 mesh, sourced from Shanghai MacLean Biotechnology Co., Ltd.;
[0063] Blowing agent: HFC-365mfc / 227ea, from Solvay, Germany;
[0064] Catalyst: o-toluenediamine polyether 401P, from Hebei Yadong Chemical Group Co., Ltd.;
[0065] Surfactant: B8444, from Evonik Degussa (China) Investment Co., Ltd.;
[0066] The photoinitiator is benzoin dimethyl ether;
[0067] Hydroxyl-terminated polydimethylsiloxane: average molecular weight 550, from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0068] Polyether polyol: PPG-700, from Shandong Bluestar Dongda Co., Ltd.;
[0069] The "parts" mentioned below are all by mass.
[0070] Embodiment 1: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following process:
[0071] Step 1, preparation of polyurethane foaming agent:
[0072] 1.1. Mix 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide and pure water in toluene, heat to 80°C, and reflux for 4 hours; slowly add allyldimethylsilyl chloride within 30 minutes, heat to 100°C, and reflux for 100 minutes; cool, wash with water, dry the organic phase, remove the solvent by rotary evaporation, dilute with toluene, and precipitate with cold methanol to obtain alkenyl-terminated oligosiloxane; the molar ratio of 1,1-dimethoxysilylcyclobutane to allyldimethylsilyl chloride is 5:1; the ratio of 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide, pure water, and toluene is 5.0g:0.010g:50mL:25mL;
[0073] Under light-proof conditions, alkenyl-terminated oligosiloxane, 2-mercaptoethanol, and 1.0% photoinitiator were mixed, mixed in toluene, stirred, and irradiated under ultraviolet light for 20 minutes, vacuum dried, petroleum ether was added, filtered, rotary evaporated, and vacuum dried to obtain hydroxyl-terminated polycarbosilane; the mass ratio of alkenyl-terminated oligosiloxane to 2-mercaptoethanol was 11.2;
[0074] 1.2. Mix fumaric acid, hydroxyl-terminated polycarbosilane and 0.10% catalyst zinc oxide, and heat to 150°C under nitrogen atmosphere, keep stirring for 30 min; heat to 220°C, react for 4 h; cool to obtain a hydroxyl-containing fumaric acid ester compound; the mass ratio of fumaric acid to hydroxyl-terminated polycarbosilane is 10:8.4;
[0075] 1.3. Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, heated to 75°C, stirred and melamine was slowly added within 30 min, and the reaction was continued for 4 h; filtered, washed, recrystallized and vacuum dried to obtain compound A; the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine and triethylamine was 3.5:1:3.0; the ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and anhydrous acetonitrile was 12 g / 100 mL;
[0076] Dissolve the hydroxy-containing fumaric acid ester compound in acetonitrile; heat to 80°C, slowly add compound A and triethylamine within 30 minutes, and react for 6 hours; cool, wash the precipitate, and vacuum dry to constant weight to obtain a phosphorus-containing polyol; the mass ratio of the hydroxy-containing fumaric acid ester compound, compound A, and triethylamine is 10.8:1:0.35; the ratio of the hydroxy-containing fumaric acid ester compound to acetonitrile is 10g / 100mL;
[0077] 1.4. Mix phosphorus-containing polyol, polyether polyol, glass fiber, blowing agent, catalyst and surfactant, stir at room temperature for 60 minutes, heat to 50°C, and stir at this temperature for 60 minutes to obtain component A; use isocyanate as component B; mix component A and component B before use to obtain a polyurethane blowing agent; the polyurethane blowing agent includes the following components by mass: 10 parts of phosphorus-containing polyol, 90 parts of polyether polyol, 130 parts of isocyanate, 1 part of triethanolamine, 1 part of glass fiber, 35 parts of blowing agent, 1.0 part of catalyst and 2 parts of surfactant;
[0078] Step 2: Take the paper core and stretch it to shape it, lay glass fiber cloth on its upper and lower surfaces to form two groups of glass fiber layers; spray polyurethane foaming agent on the surface of the upper glass fiber layer; turn it over, spray polyurethane foaming agent on the surface of the other group of glass fiber layers, mold and foam to form a PU layer; the thickness of the PU layer is 5mm and the weight is 330g / m 2 The molding process is as follows: mold temperature 115°C, pressure 10MPa, and duration 50s; the surface patch is adhered to the surface of the PU layer located above by polyurethane glue to obtain a polyurethane spray cover plate.
[0079] Embodiment 2: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following process:
[0080] Step 1, preparation of polyurethane foaming agent:
[0081] 1.1. Mix 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide and pure water in toluene, heat to 82°C, and reflux for 4.5 hours; slowly add 7-octenyldimethylsilyl chloride within 30 minutes, heat to 100°C, and reflux for 120 minutes; cool, wash with water, dry the organic phase, remove the solvent by rotary evaporation, dilute with toluene, and precipitate with cold methanol to obtain alkenyl-terminated oligosiloxane; the molar ratio of 1,1-dimethoxysilylcyclobutane to 7-octenyldimethylsilyl chloride is 5.5:1; the ratio of 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide, pure water, and toluene is 5.1g:0.011g:50mL:25mL;
[0082] Under light-proof conditions, alkenyl-terminated oligosiloxane, 2-mercaptoethanol, and 1.2% photoinitiator were mixed in toluene, stirred, and irradiated under ultraviolet light for 25 minutes, vacuum dried, petroleum ether was added, filtered, rotary evaporated, and vacuum dried to obtain hydroxyl-terminated polycarbosilane; the mass ratio of alkenyl-terminated oligosiloxane to 2-mercaptoethanol was 13.6;
[0083] 1.2. Mix fumaric acid, hydroxyl-terminated polycarbosilane and 0.12% catalyst zinc oxide, and heat to 155°C under nitrogen atmosphere, keep stirring for 45 minutes; heat to 230°C, react for 5 hours; cool to obtain a hydroxyl-containing fumaric acid ester compound; the mass ratio of fumaric acid to hydroxyl-terminated polycarbosilane is 10:10.5;
[0084] 1.3. Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, heated to 80°C, stirred and melamine was slowly added within 30 min, and the reaction was continued for 4.5 h; filtered, washed, recrystallized and vacuum dried to obtain compound A; the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine and triethylamine was 3.8:1:3.2; the ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and anhydrous acetonitrile was 12 g / 100 mL;
[0085] Dissolve the hydroxy-containing fumaric acid ester compound in acetonitrile; heat to 85°C, slowly add compound A and triethylamine, add within 30 minutes, and react for 6.5 hours; cool, wash the precipitate, and vacuum dry to constant weight to obtain a phosphorus-containing polyol; the mass ratio of the hydroxy-containing fumaric acid ester compound, compound A, and triethylamine is 12.0:1:0.42; the ratio of the hydroxy-containing fumaric acid ester compound to acetonitrile is 10 g / 100 mL;
[0086] 1.4. Mix phosphorus-containing polyol, polyether polyol, glass fiber, blowing agent, catalyst and surfactant, stir at room temperature for 75 minutes, heat to 55°C, and stir at this temperature for 90 minutes to obtain component A; use isocyanate as component B; mix component A and component B before use to obtain a polyurethane blowing agent; the polyurethane blowing agent includes the following components by mass: 20 parts of phosphorus-containing polyol, 80 parts of polyether polyol, 145 parts of isocyanate, 1.5 parts of triethanolamine, 2 parts of glass fiber, 38 parts of blowing agent, 1.2 parts of catalyst and 1.5 parts of surfactant;
[0087] Step 2: Take the paper core and stretch it to shape it, lay glass fiber cloth on its upper and lower surfaces to form two groups of glass fiber layers; spray polyurethane foaming agent on the surface of the upper glass fiber layer; turn it over, spray polyurethane foaming agent on the surface of the other group of glass fiber layers, mold and foam to form a PU layer, the thickness of the PU layer is 5mm, and the weight is 325g / m 2 The molding process is as follows: mold temperature 110°C, pressure 8MPa, and duration 45s; the surface patch is adhered to the surface of the PU layer located above by polyurethane glue to obtain a polyurethane spray cover plate.
[0088] Embodiment 3: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following process:
[0089] Step 1, preparation of polyurethane foaming agent:
[0090] 1.1. Mix 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide and pure water in toluene, heat to 85°C, and reflux for 5 hours; slowly add 1-alkenyl undecyl dimethyl silyl chloride within 30 minutes, heat to 100°C, and reflux for 150 minutes; cool, wash with water, dry the organic phase, remove the solvent by rotary evaporation, dilute with toluene, and precipitate with cold methanol to obtain alkenyl-terminated oligosiloxane; the molar ratio of 1,1-dimethoxysilylcyclobutane to 1-alkenyl undecyl dimethyl silyl chloride is 6:1; the ratio of 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide, pure water, and toluene is 5.2g:0.012g:50mL:25mL;
[0091] Under light-proof conditions, alkenyl-terminated oligosiloxane, 2-mercaptoethanol, and 1.5% photoinitiator were mixed, mixed in toluene, stirred, and irradiated under ultraviolet light for 30 minutes, vacuum dried, petroleum ether was added, filtered, rotary evaporated, and vacuum dried to obtain hydroxyl-terminated polycarbosilane; the mass ratio of alkenyl-terminated oligosiloxane to 2-mercaptoethanol was 14.6;
[0092] 1.2. Mix fumaric acid, hydroxyl-terminated polycarbosilane and 0.15% catalyst zinc oxide, and heat to 160°C under nitrogen atmosphere, keep warm and stir for 60 min; heat to 240°C, react for 6 h; cool to obtain a hydroxyl-containing fumaric acid ester compound; the mass ratio of fumaric acid to hydroxyl-terminated polycarbosilane is 10:12.5;
[0093] 1.3. Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, heated to 85°C, stirred and melamine was slowly added within 30 min, and the reaction was continued for 5 h; filtered, washed, recrystallized and vacuum dried to obtain compound A; the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine and triethylamine was 4.0:1:3.5; the ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and anhydrous acetonitrile was 12 g / 100 mL;
[0094] Dissolve the hydroxy-containing fumaric acid ester compound in acetonitrile; heat to 90°C, slowly add compound A and triethylamine within 30 minutes, and react for 7 hours; cool, wash the precipitate, and vacuum dry to constant weight to obtain a phosphorus-containing polyol; the mass ratio of the hydroxy-containing fumaric acid ester compound, compound A, and triethylamine is 13.3:1:0.50; the ratio of the hydroxy-containing fumaric acid ester compound to acetonitrile is 10 g / 100 mL;
[0095] 1.4. Mix phosphorus-containing polyol, polyether polyol, glass fiber, blowing agent, catalyst and surfactant, stir at room temperature for 90 minutes, heat to 60°C, and stir for 120 minutes to obtain component A; use isocyanate as component B; mix component A and component B before use to obtain a polyurethane blowing agent; the polyurethane blowing agent includes the following components by mass: 30 parts of phosphorus-containing polyol, 70 parts of polyether polyol, 160 parts of isocyanate, 2 parts of triethanolamine, 3 parts of glass fiber, 40 parts of blowing agent, 1.5 parts of catalyst and 1 part of surfactant;
[0096] Step 2: Take the paper core and stretch it to shape it, lay glass fiber cloth on its upper and lower surfaces to form two groups of glass fiber layers; spray polyurethane foaming agent on the surface of the upper glass fiber layer; turn it over, spray polyurethane foaming agent on the surface of the other group of glass fiber layers, mold and foam to form a PU layer; the thickness of the PU layer is 5mm and the weight is 327g / m 2 The molding process is as follows: mold temperature 105°C, pressure 5MPa, and duration 40s; the surface patch is adhered to the surface of the PU layer located above by polyurethane glue to obtain a polyurethane spray cover plate.
[0097] Comparative Example 1: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following processes:
[0098] Step 1, preparation of polyurethane foaming agent:
[0099] 1.1. Mix fumaric acid, polyether polyol and 0.10% catalyst zinc oxide, and heat to 150°C under nitrogen atmosphere, keep warm and stir for 30 min; heat to 220°C, react for 4 h; cool to obtain hydroxy-containing fumaric acid ester compound; the mass ratio of fumaric acid to polyether polyol is 10:8.4;
[0100] Steps 1.2 / 1.3 and step 2 are the same as steps 1.3 / 1.4 and step 2 in Example 1 to obtain a polyurethane spray-coated cover plate.
[0101] Comparative Example 2: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following processes:
[0102] Step 1, preparation of polyurethane foaming agent:
[0103] Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, heated to 75°C, stirred and melamine was slowly added within 30 minutes, and the reaction was carried out for 4 hours; filtered, washed, recrystallized, and vacuum dried to obtain compound A; the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine, and triethylamine was 3.5:1:3.0; the ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and anhydrous acetonitrile was 12 g / 100 mL;
[0104] Dissolve the hydroxyl-terminated polydimethylsiloxane in acetonitrile; heat to 80°C, slowly add compound A and triethylamine, add within 30 minutes, and react for 6 hours; cool, wash the precipitate, and vacuum dry to constant weight to obtain a phosphorus-containing polyol; the mass ratio of hydroxyl-terminated polydimethylsiloxane, compound A, and triethylamine is 2.3:1:0.08; the ratio of hydroxy-containing fumaric ester compound and acetonitrile is 10g / 100mL;
[0105] Step 1.2 and step 2 are the same as step 1.4 and step 2 in Example 1 to obtain a polyurethane spray-coated cover plate.
[0106] Comparative Example 3: A preparation process of a glass fiber reinforced polyurethane spray cover plate, comprising the following processes:
[0107] Step 1, preparation of polyurethane foaming agent:
[0108] The polyurethane foaming agent includes the following components by mass: 100 parts of polyether polyol, 130 parts of isocyanate, 1 part of triethanolamine, 1 part of glass fiber, 35 parts of foaming agent, 1.0 part of catalyst, and 2 parts of surfactant;
[0109] Step 2 is the same as step 2 in Example 1 to obtain a polyurethane spray-coated cover plate.
[0110] Experiment: The PU layers and polyurethane spray-coated cover plates obtained in Examples 1-3 and Comparative Examples 1-3 were taken to prepare samples, and their properties were tested respectively and the test results were recorded:
[0111] Flame retardant performance test: GB / T 2406.2 is used as the reference standard, and an oxygen index instrument is used to detect the limiting oxygen index of the PU layer sample. The sample size is 100mm×10mm×10mm;
[0112] Compression performance test: GB / T 8813 is used as the reference standard to test the compressive strength of the PU layer sample. The compression speed is 1mm / min. At a temperature of 23±2℃, the compressive stress of the sample under a relative deformation of 10% is taken as the compressive strength. The sample size is 50mm×50mm×50mm;
[0113] Shear performance test: Taking GB / T 10007 as the reference standard, an electronic universal testing machine was used to test the shear strength of the PU layer sample. The sample size was 250mm×50mm×25mm, and the shear speed was 1mm / min.
[0114] Limiting oxygen index LOI (%) Shear strength(MPa) Compression strength(MPa) Example 1 28.2 0.78 1.08 Example 2 29.1 0.80 1.11 Example 3 30.7 0.85 1.17 Comparative Example 1 26.3 0.71 1.00 Comparative Example 2 25.9 0.65 0.91 Comparative Example 3 22.4 0.61 0.85
[0115] According to the data in the above table, we can clearly draw the following conclusions:
[0116] The polyurethane sprayed cover plates obtained in Examples 1-3 are compared with the polyurethane sprayed cover plates obtained in Comparative Examples 1-3. The test results show that:
[0117] Compared with the comparative example, the PU layer obtained in Examples 1-3 has higher limiting oxygen index (LOI), bending strength and shear strength data. It can be seen that the polyurethane foam formed by the prepared polyurethane foaming agent obtained in Examples 1-3 after spraying has better mechanical strength and flame retardant properties, and the polyurethane spray cover plate obtained in Examples 1-3 can achieve improvement in its strength and flame retardant ability.
[0118] Compared with Example 1, the hydroxy-containing fumaric acid ester compound in the PU layer of Comparative Example 1 is made of fumaric acid and polyether polyol, and the hydroxyl-terminated polycarbosilane is replaced by polyether polyol, and does not contain flame retardant element silicon and rigid silicon-based cyclobutane, so that the strength and limiting oxygen index data of the PU layer are reduced. The phosphorus-containing polyol in the PU layer of Comparative Example 2 is made of hydroxyl-terminated polydimethylsiloxane and compound A, and does not contain fumaric acid and polycarbosilane structure, so that the strength of the PU layer is further reduced. The PU layer of Comparative Example 3 does not use the phosphorus-containing polyol component, and its PU layer strength and limiting oxygen index data are the lowest. It can be seen that the setting of the polyurethane foaming agent component and its process of the present invention can promote the improvement of the mechanical strength and flame retardant properties of the PU layer, and the obtained polyurethane spray cover can have more excellent strength and flame retardant performance.
[0119] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0120] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of a glass fiber reinforced polyurethane spray cover plate, characterized in that: Including the following processes: Take the paper core and stretch it to shape it, and lay glass fiber cloth on its upper and lower surfaces to form two sets of glass fiber layers; Spray polyurethane foaming agent on the surface of the upper glass fiber layer; turn over, spray polyurethane foaming agent on the surface of another group of glass fiber layers, mold, foam, and form a PU layer; The surface patch is adhered to the surface of the PU layer located above by using polyurethane glue to obtain a polyurethane spray-coated cover plate; The polyurethane foaming agent component contains phosphorus-containing polyols, which include the following components: 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine, fumaric acid and hydroxyl-terminated polycarbosilane.
2. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 1, characterized in that: The polyurethane foaming agent is prepared by the following process: The phosphorus-containing polyol, polyether polyol, glass fiber, foaming agent, catalyst and surfactant are mixed, stirred at room temperature for 60 to 90 minutes, heated to 50 to 60° C., and stirred at this temperature for 60 to 120 minutes to obtain component A; Isocyanate is used as component B; Before use, component A and component B are mixed to obtain a polyurethane foaming agent.
3. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 2, characterized in that: The polyurethane foaming agent comprises the following components by weight: 10 to 30 parts of phosphorus-containing polyol, 70 to 90 parts of polyether polyol, 130 to 160 parts of isocyanate, 1 to 2 parts of triethanolamine, 1 to 3 parts of glass fiber, 35 to 40 parts of foaming agent, 1.0 to 1.5 parts of catalyst, and 1 to 2 parts of surfactant.
4. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 2, characterized in that: The phosphorus-containing polyol is prepared by the following process: Under nitrogen atmosphere, 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, anhydrous acetonitrile and triethylamine were mixed, the temperature was raised to 75-85° C., melamine was slowly added with stirring within 30 minutes, and the reaction was carried out for 4-5 hours to obtain compound A; Dissolving the hydroxyfumaropimarate-containing compound in acetonitrile; The temperature was raised to 80-90°C, and compound A and triethylamine were slowly added within 30 minutes. The reaction was continued for 6-7 hours to obtain a phosphorus-containing polyol.
5. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 4, characterized in that: The hydroxy-containing fumaric pimarate compound is prepared by the following process: Mix fumaric acid, hydroxyl-terminated polycarbosilane and zinc oxide, and heat to 150-160° C. under nitrogen atmosphere, and stir for 30-60 min; heat to 220-240° C., and react for 4-6 h to obtain a hydroxyl-containing fumaric acid ester compound.
6. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 5, characterized in that: The hydroxyl-terminated polycarbosilane is prepared by the following process: 1,1-dimethoxysilylcyclobutane, tetramethylammonium hydroxide and pure water are mixed in toluene, heated to 80-85°C, and refluxed for 4-5 hours; alkenyldimethylsilyl chloride is slowly added within 30 minutes, heated to 100°C, and refluxed for 100-150 minutes to obtain alkenyl-terminated oligosiloxane; Under light-proof conditions, alkenyl-terminated oligosiloxane, 2-mercaptoethanol and a photoinitiator are mixed in toluene, stirred and irradiated under an ultraviolet lamp for 20 to 30 minutes to obtain a hydroxyl-terminated polycarbosilane.
7. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 4, characterized in that: The molar ratio of the 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, melamine and triethylamine is (3.5-4.0):1:(3.0-3.5).
8. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 4, characterized in that: The mass ratio of the hydroxy-fumaropimaric acid ester compound, compound A and triethylamine is (10.8-13.3):1:(0.35-0.50).
9. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 5, characterized in that: The mass ratio of the fumaric acid to the hydroxyl-terminated polycarbosilane is 10:(8.4-12.5).
10. The process for preparing a glass fiber reinforced polyurethane spray cover plate according to claim 6, characterized in that: The molar ratio of the 1,1-dimethoxysilycyclobutane to alkenyldimethylchlorosilane is (5-6):1.
Citation Information
Cited By
High-strength honeycomb paper core cover plate and preparation process thereof
CN120134717A
Online detection and respraying method for spraying forming of polyurethane composite material
CN122649255A
Polyurethane composite spray forming online detection and supplementary spraying method
CN122649255B