Laminated glass having regions with different refractive indices

By using films A and film B with different refractive indices in the glass laminate, laminated glass is solved, and the problem of low quality of PVB intermediate layer in the prior art is achieved, and the effect of detecting authenticity and improving optical characteristics is achieved.

CN118977491APending Publication Date: 2024-11-19KURARAY EURO GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411200452.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-27
Filing Date
2020-02-21
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The polyvinyl butyral (PVB) intermediate layer used in existing glass laminates has low quality, making it difficult to detect whether a real PVB intermediate layer is used, affecting the authenticity of the product.

Method used

Two separate films with different refractive indices are used as intermediate layers, and laminated glass is formed by bonding the adhesive film. The difference in refractive indices between film A and film B makes the pattern visible when illuminated, achieving the purpose of detection.

Benefits of technology

The visible pattern is formed through films A and film B with different refractive indices, which solves the problem of detecting the real PVB intermediate layer, improves the transparency and opacity of the product, is suitable for laminates of thin glass sheets, and enhances optical characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977491A_ABST
    Figure CN118977491A_ABST
Patent Text Reader

Abstract

The present invention relates to laminated glass comprising two sheets of glass bonded by an adhesive film comprising: at least one film B comprising a polyvinyl acetal PB and at least one plasticizer WB; and at least one region A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, characterized in that the refractive index of the film A and the film B differs by at least 0.0002.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to laminated glass, in particular windscreens or laminates for use in construction, which are provided with different refractive indices when illuminated from their edges or sides. Technical Background

[0002] Polyvinyl butyral (PVB) interlayers used in glass laminates are often supplied in low quality. However, some of these interlayers are laminated with glass sheets to form the final glass, making it difficult for the end customer to tell whether the genuine product has been used in the glass. Summary of the Invention

[0003] Therefore, the object of the present invention is to provide a laminate that makes it possible to detect whether a genuine PVB interlayer is used. The inventors have found that this object is achieved by using an interlayer comprising two separate films with different refractive indices. When illuminated from its edge or side, the pattern can be made visible like a watermark.

[0004] The subject of the present invention is therefore a laminated glass comprising two sheets of glass joined by an adhesive film comprising: at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB; and at least one area A comprising polyvinyl acetal PA and optionally at least one plasticizer WA, characterised in that the refractive indices of films A and B differ by at least 0.0002.

[0005] Figures 1 to 6 The invention is illustrated along with the possible patterns detected by two films with different refractive indices when illuminated.

[0006] The pattern of film A having a different refractive index than film B can be applied to film B by various techniques known to those skilled in the art. Film A can be manufactured by extrusion and then cut or stamped into shape and co-laminated with film B. Alternatively, PVB can be printed (e.g., 3D printed) onto film B, or printed onto a sheet of glass and then co-laminated to film B to form film A.

[0007] Preferably, the thickness of region A is at least 5 μm.

[0008] In a first embodiment, the laminated glass has two surface regions and at least three edge regions, and wherein the refractive indices of region A and film B differ by at least 0.0002 when the laminated glass is illuminated from one of the edge regions or the surface regions.

[0009] In a second embodiment, at least one of the edge region or the surface region is provided with lighting or daylight.

[0010] In a third embodiment, the amount of plasticizer WA in area A is less than 45% by weight, and the amount of plasticizer WB in film B is less than 45% by weight, before bonding the two glass sheets.

[0011] In a fifth embodiment, the area A is provided by printing onto or into the film B a melt comprising polyvinyl acetal PA and optionally at least one plasticizer WA.

[0012] In a sixth embodiment, the areas A are provided by combining a film B with a cut-out or punched pattern of a film A comprising polyvinyl acetal PA and optionally at least one plasticizer WA.

[0013] In a seventh embodiment, one or more areas A are sandwiched between two films B comprising identical or different polyvinyl acetals PB and at least one plasticizer WB.

[0014] In an eighth embodiment, region A includes an inorganic filler, a pigment, or a dye.

[0015] In the ninth first embodiment, the film B includes an inorganic filler, a pigment, or a dye.

[0016] In the tenth embodiment, the ratio of the thickness of the region A to the film B is between 0.002 and 1, preferably between 0.002 and 0.2.

[0017] In an eleventh embodiment, the film B comprises at least two layers, wherein the amount of plasticizer WB in the layers differs by at least 2% by weight.

[0018] In the twelfth embodiment, the film B has a wedge-shaped thickness profile.

[0019] Another object of the present invention is a process for producing laminated glass by bonding two sheets of glass with an adhesive film, the adhesive film comprising: at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB; and at least one area A comprising polyvinyl acetal PA and optionally at least one plasticizer WA, wherein the refractive indices of films A and B differ by at least 0.0002, by printing a melt comprising polyvinyl acetal PA and optionally at least one plasticizer WA onto or into film B.

[0020] Hereinafter, the term "before lamination" refers to the state of film A and film B before they come into contact with each other. For example, the term refers to the composition of each film formed separately and wound onto separate rolls. The term "before lamination" refers to the state of the layers or films before they are combined during the lamination process of laminated glass or before a stack is constructed from the layers used for lamination.

[0021] The term "region A" refers to a region having a continuous or discontinuous surface comprising a mixture comprising polyvinyl acetal PA and optionally at least one plasticizer WA. Preferably, region A is provided by a film. It should be noted that throughout this application, the terms "film A" and "region A" are used as synonyms.

[0022] The present invention is also advantageous for laminates comprising thin glass sheets, since sintering enamel on thin glass is even more prone to producing off-specification curved sheets with optical defects. In preferred embodiments of the present invention, at least one of the glass sheets has a thickness of less than 2.1 mm, such as 1.8 mm, less than 1.8 mm; less than 1.6 mm; less than 1.4 mm; less than 1.0 mm; or less than 0.9 mm.

[0023] Area A

[0024] The laminate according to the invention may comprise one or more films A, but at least one film A is oriented adjacent to the glass surface of the laminated glass according to the invention. It is also possible to apply film A to both glass surfaces, so that a laminated glass laminate having the layer sequence glass / film A / film B / film A / glass is provided.

[0025] The dry film thickness of the printed area is between 1 and 50 μm, depending on the printing technique and the desired opacity. Typically, the dry film thickness is between 10 and 30 μm. A sufficiently high total dry film thickness can be achieved by repeating the successive printing / coating steps to build up the ink layer.

[0026] The thickness ratio of film A to film B in the initial state before lamination may be less than 0.2.

[0027] The thickness of film A in its initial state before lamination is 10-250 μm, preferably 20-160 μm, preferably 30-120 μm, preferably 40-100 μm, and most preferably 50-80 μm. This thickness range does not include additional printed / coated layers on the film. In laminated glass, the thickness of the film can be increased by transferring plasticizers from film B.

[0028] Film A is produced separately from film B (eg, extrusion or solvent casting) and is completely free of plasticizer or contains a sufficiently small proportion of plasticizer so as not to adversely affect subsequent functionalization and processing.

[0029] Since film A will preferably be in direct contact with one of the inner surfaces of the laminated glass, it is desirable to control its adhesion to an intermediate level in order to achieve satisfactory penetration resistance as mandated for different glass locations in motor vehicles, as specified in various safety glass standards, such as ECE 43R. To this end, film A may contain alkali metal ions and / or alkaline earth metal ions to adjust their level of adhesion to the glass (so-called anti-adhesion additives).

[0030] Potassium, sodium, or lithium are preferred as alkali metal ions. Preferred concentration ranges for alkali metal ions are: 7-210 ppm, preferably 14-140 ppm, and more preferably 21-140 ppm for lithium; 23-690 ppm, preferably 46-460 ppm, and more preferably 69-460 ppm for sodium; and 39-1170 ppm, preferably 78-780 ppm, and more preferably 117-780 ppm for potassium. Furthermore, it is preferred to add the alkali metal ions in the form of carboxylates having 1 to 10 carbon atoms. Potassium acetate is particularly preferred as an adhesion control agent.

[0031] The total amount of alkali metal salt can be as low as 0.005% by weight based on the weight of membrane A. Preferred ranges for alkali metal salt are 0.01%-0.1%; 0.02–0.08%; 0.03–0.06%, each weight % based on the weight of membrane A.

[0032] The film A used in the laminate of the present invention may additionally comprise alkaline earth ions, but due to their limited effect on adhesion, only small amounts should be used compared to alkali ions. In a first embodiment of the present invention, film A comprises 0 to 20 ppm of alkaline earth ions, preferably 0 to 5 ppm.

[0033] However, it is known that when the plasticized PVB film is facing two glass sheets with different surface chemical properties, alkaline earth ions have a balanced adhesion effect. Therefore, in a second embodiment of the present invention, film A includes 5-20ppm alkaline earth ions. Alkaline earth ions can be added in the form of carboxylates with 1 to 10 carbon atoms. Especially preferred is magnesium acetate as an auxiliary adhesion control agent. In this embodiment, the ratio of alkali ions to alkaline earth ions (in ppm) is preferably at least higher than 1, especially higher than 5, and more preferably higher than 10 in film A.

[0034] Instead of the amount of alkali ions and alkaline earth ions, the alkalinity titer of membranes A and B can be used to characterize the amount of anti-adherent agent (i.e., alkali salt and alkaline earth salt) in the membranes. The alkalinity titer of membrane A can be higher than 10, higher than 20, higher than 40, higher than 50, higher than 80, higher than 90, and preferably higher than 100, with a maximum value of 500 in each case. The alkalinity titer of membrane B is preferably lower than that of membrane A, and more particularly, the difference between alkalinity titer (membrane A) - alkalinity titer (membrane B) is greater than 2, 6, and preferably greater than 10 AT units.

[0035] In order to avoid haze, the amount of chloride ions and / or nitrate ions and / or sulfate ions in membrane A may be reduced.

[0036] The chloride content of membrane A may therefore be less than 150 ppm, preferably less than 100 ppm, and in particular less than 50 ppm. In the ideal case, the chloride content of membrane A is less than 10 ppm or even 0 ppm.

[0037] The nitrate content of membrane A may optionally be less than 150 ppm, preferably less than 100 ppm, and in particular less than 50 ppm. Ideally, the nitrate content of membrane A is less than 10 ppm or even 0 ppm.

[0038] Alternatively again, the sulfate content of membrane A may be less than 150 ppm, preferably less than 100 ppm, and in particular less than 50 ppm. Ideally, the sulfate content of membrane A is less than 10 ppm or even 0 ppm.

[0039] Membrane B

[0040] Film B can be any plasticized PVB film known in the art. In the initial state before lamination and / or in the stack prepared for lamination between glass sheets, films A and B can contain a single plasticizer, as well as mixtures of plasticizers with both different and identical compositions. The term "different compositions" refers to both the type of plasticizer in the mixture and its proportion. After lamination (i.e., in the finished laminated glass), films A and B preferably have the same plasticizers WA and WB. However, in a preferred variant, film A does not contain any plasticizer in its initial state and contains a balanced amount of plasticizer WB after lamination.

[0041] The plasticizer-containing film B used according to the invention contains at least 22% by weight, such as 22.0-45.0% by weight, preferably 25.0-32.0% by weight and in particular 26.0-30.0% by weight of plasticizer in the starting state before lamination.

[0042] The film A used according to the present invention may contain less than 22% by weight (such as 21.9% by weight), less than 18% by weight, less than 16% by weight, less than 12% by weight, less than 8% by weight, less than 4% by weight, less than 2% by weight, less than 1% by weight of plasticizer in the starting state before lamination, or even no plasticizer (0.0% by weight). In a preferred embodiment of the present invention, the film A with a low plasticizer content preferably contains 0.0-8% by weight of plasticizer, most preferably 0-4wght% of plasticizer.

[0043] Film A or film B preferably comprises polyvinyl acetal with a proportion of polyvinyl acetate groups, the proportion being the same or different and being from 0.1 to 20 mol %, preferably from 0.5 to 3 mol %, or from 5 to 8 mol %.

[0044] The thickness of the membrane B in the initial state is 450-2500 μm, preferably 600-1000 μm, preferably 700-900 μm. In the present invention, a plurality of membranes B can be used, which are either stacked on top of each other or separated by membranes A.

[0045] If film B is stretched and / or additionally adapted in a curved manner to the shape of the screen (eg windshield) before producing the sandwich structure, the specified thickness at the time of lamination can be reduced again by up to 20%.

[0046] Polyvinyl acetal

[0047] Films A and B used according to the invention comprise polyvinyl acetals which are produced by acetalisation of polyvinyl alcohol or ethylene vinyl alcohol copolymers.

[0048] The film may comprise polyvinyl acetals, each having a different polyvinyl alcohol content, degree of acetalization, residual acetate content, ethylene proportion, molecular weight and / or chain length of the aldehyde of the acetal group.

[0049] In particular, the aldehyde or ketone compounds used to produce polyvinyl acetals can be linear or branched (that is to say of the "normal (n)" or "iso (iso)" type), containing 2 to 10 carbon atoms, which results in corresponding linear or branched acetal groups. Polyvinyl acetals are therefore referred to as "polyvinyl alcohol (iso) acetals" or "polyvinyl alcohol (n) acetals".

[0050] The polyvinyl acetal used according to the invention is produced in particular by the reaction of at least one polyvinyl alcohol with one or more aliphatic unbranched ketone compounds containing 2 to 10 carbon atoms. For this purpose, n-butyraldehyde is preferably used.

[0051] The polyvinyl alcohol or ethylene vinyl alcohol copolymer used to produce the polyvinyl acetal in membrane A or membrane B may be the same or different, pure or a mixture of polyvinyl alcohols or ethylene vinyl alcohol copolymers having different degrees of polymerization or hydrolysis.

[0052] The polyvinyl acetate content of the polyvinyl acetal in film A or film B can be adjusted by using polyvinyl alcohol or ethylene vinyl alcohol copolymer saponified to an appropriate degree. The polarity of the polyvinyl acetal is influenced by the polyvinyl acetate content, thereby also changing the plasticizer compatibility and mechanical strength of the corresponding layer. It is also possible to acetalize the polyvinyl alcohol or ethylene vinyl alcohol copolymer using a mixture of various aldehyde or ketone compounds.

[0053] Film A or film B preferably comprises polyvinyl acetal with a proportion of polyvinyl acetate groups, the proportion being the same or different and being from 0.1 to 20 mol %, preferably from 0.5 to 3 mol %, or from 5 to 8 mol %.

[0054] The polyvinyl alcohol content of the polyvinyl acetal PA used in film A may be between 6-26% by weight, between 8-24% by weight, between 10-22% by weight, between 12-21% by weight, between 14-20% by weight, between 16-19% by weight, and preferably between 16 and 21% by weight or between 10-16% by weight.

[0055] Independently of film A, the polyvinyl alcohol content of the polyvinyl acetal PB used in film B may be between 14-26% by weight, between 16-24% by weight, between 17-23% by weight, and preferably between 18 and 21% by weight.

[0056] In a preferred embodiment of the invention, film A comprises polyvinyl acetal PA having a proportion of vinyl alcohol groups from 6 to 26% by weight, and film B comprises polyvinyl acetal B having a proportion of vinyl alcohol groups from 14 to 26% by weight.

[0057] plasticizers

[0058] The film A and / or the film B used according to the invention may contain one or more compounds selected from the following group as plasticizers:

[0059] - esters of polyvalent aliphatic or aromatic acids, for example, dialkyl adipates such as dihexyl adipate, dioctyl adipate, hexyl cyclohexyl adipate, a mixture of heptyl and nonyl adipate, diisononyl adipate, heptononyl adipate, and esters of adipic acid with alicyclic ester alcohols or ester alcohols containing ether compounds, dialkyl sebacates such as dibutyl sebacate, and also esters of sebacic acid with alicyclic ester alcohols or ester alcohols containing ether compounds, phthalates such as butyl benzyl phthalate or di-2-butoxyethyl phthalate.

[0060] - esters or ethers of polyvalent aliphatic or aromatic alcohols or oligoether glycols having one or more unbranched or branched aliphatic or aromatic substituents, for example, esters of glycerol, diethylene glycol, triethylene glycol or tetraethylene glycol with linear or branched aliphatic or alicyclic carboxylic acids; examples of the latter group include diethylene glycol bis-(ethyl 2-hexanoate), triethylene glycol bis-(ethyl 2-hexanoate), triethylene glycol bis-(ethyl 2-butyrate), tetraethylene glycol bis-n-heptanoate, triethylene glycol bis-n-heptanoate, triethylene glycol bis-n-hexanoate, tetraethylene glycol dimethyl ether and / or dipropylene glycol benzoate;

[0061] - phosphoric acid esters with aliphatic or aromatic ester alcohols, such as tris(2-ethylhexyl) phosphate (TOF), triethyl phosphate, diphenyl-2-ethylhexyl phosphate and / or tricresyl phosphate;

[0062] - Esters of citric acid, succinic acid and / or fumaric acid.

[0063] By definition, plasticizers are organic liquids with a high boiling point. For this reason, further types of organic liquids with boiling points above 120° C. can also be used as plasticizers.

[0064] Film A, and also film B in the variant in which the plasticizer WA is initially present in film A, particularly preferably comprise diisononyl-1,2-cyclohexanedicarboxylate (DINCH) or triethylene glycol bis-2-ethylhexanoate (3GO or 3G8) as plasticizer.

[0065] The film B may consist of at least two sub-films B′ and B″, which have different plasticizer contents.

[0066] Furthermore, membranes A and B may contain further additives, such as residual amounts of water, UV absorbers, antioxidants, adhesion regulators, fluorescent brighteners or fluorescent additives, stabilizers, colorants, processing aids, inorganic or organic nanoparticles, pyrogenic silicic acid and / or surface-active substances.

[0067] In particular, membrane B may comprise 0.001 to 0.1% by weight of alkali metal and / or alkaline earth salts of carboxylic acids as adhesion control agents.Preferably, membrane B comprises magnesium ions in an amount of at least 10 ppm, preferably 20 ppm and most preferably 30 ppm.

[0068] Lamination process

[0069] The invention also relates to a method for producing the described glass laminate, wherein film A is positioned on a glass sheet, then covered by at least one film B, and then a second glass sheet is applied.

[0070] Alternatively, it is possible to position the film B on a glass sheet, which is then covered by at least one film A, and to apply a second glass sheet.

[0071] The invention further relates to a method for producing laminated glass, wherein a stack comprising at least one film A and at least one film B is provided, the stack is positioned on a first glass sheet, and then a second glass sheet is applied.

[0072] According to the invention, it is possible to first melt film A onto the glass sheet over the entire area or locally by elevated temperature and then cover it with film B. Alternatively, films A and B can be positioned together between two glass sheets and melted at elevated temperature.

[0073] The lamination step for producing laminated glass is preferably carried out such that films A and B are positioned between two glass sheets and the layered body thus produced is pressed under elevated or reduced pressure and elevated temperature to form the laminate.

[0074] For laminating the layered bodies, methods familiar to the person skilled in the art can be used both with and without previously produced prelaminates.

[0075] The so-called "autoclave process" is carried out over approximately 2 hours at an elevated pressure of approximately 10 to 15 bar and a temperature of 100 to 150° C. The vacuum bag or vacuum ring method (e.g. according to EP 1 235 683 B1) operates at approximately 200 mbar and 130 to 145° C.

[0076] Vacuum laminators are also available. These consist of a chamber that can be heated and evacuated, in which laminated glass can be laminated within 30-60 minutes. Reduced pressures from 0.01 to 300 mbar and temperatures from 100 to 200°C, particularly 130–160°C, have proven their worth in practice.

[0077] In the simplest case, to produce a laminated glass laminate, film A or film B is positioned on a glass sheet, and simultaneously or subsequently, another film B or film A is positioned. A second glass sheet is then applied, and the glass film laminate is produced. Excess air can then be removed using any pre-lamination method known to those skilled in the art. Here, too, the layers are initially lightly adhesively bonded to each other and to the glass.

[0078] The glass film laminate can then be subjected to an autoclave process. Film A is preferably positioned on the first glass sheet and covered with the thicker film B before the second glass sheet is applied. This method can be implemented in many conceivable and, in principle, practical variations. For example, film A can be easily removed from a roll of appropriate width, while film B is pre-cut to the size of the laminated glass to be produced. This is particularly advantageous in the case of windshields and other automotive glass parts. In such cases, it is particularly advantageous to additionally stretch the thicker film B before cutting it. This allows for more economical use of the films or, in cases where film B has a bright color tint, allows its curvature to be adapted to the upper sheet edge.

[0079] In the automotive sector, in particular for the production of windshields, film A and / or film B can be provided with a colored area, such as an ink ribbon, in the upper region of the film. For this purpose, the upper part of film B can be coextruded with a suitably colored polymer melt.

[0080] According to the invention, the film B can therefore have a color tone which has been adapted to the geometry of the windshield in a preceding process step, in particular by the above-described shaping process.

[0081] It is also possible for film B to have a wedge-shaped thickness profile. The laminated glass laminate according to the invention achieves a wedge-shaped thickness profile even with the plane-parallel thickness profile of film A and can be used in motor vehicle windshields for HUD displays.

[0082] Alternatively, film B may comprise at least two layers, wherein the amount of plasticizer WB in the layers differs by at least 2% by weight.For sound reduction purposes, film B comprises 3 layers, wherein the core layer is softer due to a higher plasticizer content.

[0083] In the simplest case, film B is a commercially available PVB film, with or without an ink ribbon and with or without a wedge-shaped thickness profile. Film B can also be used as a colored film, with dispersed nanoparticles for IR protection. Of course, film B can also be a film with acoustical functions, thereby achieving further improved sound insulation properties through its combination with film A. Of course, film B can also incorporate multiple of the aforementioned functions.

[0084] Film A is typically produced by extrusion using a cast film line or in the form of a blown film. Here, the surface roughness can also be produced by controlled melt fracture or by means of a cast film process that additionally uses structured cooling rolls and / or structured back rolls. Alternatively, a solvent casting process can be used to produce film A before functionalization and to be used in the described permeation-resistant glass laminates. The film used according to the invention preferably has a single-sided surface structure with a roughness Rz of 0 to 25 μm, preferably Rz of 1 to 20 μm, particularly preferably Rz of 3 to 15 μm, and in particular Rz of 4 to 12 μm. It is particularly preferred if the side of film A that comes into contact with the glass sheet has a surface roughness Rz of no more than 20% of its thickness.

[0085] Example

[0086] Polysmooth PVB filament from Polymaker (with a refractive index of 1,48970) was 3D-printed onto glass using a Raise3DN2 Plus 3D printer at a nozzle temperature of 215°C, a heated build plate of 70°C, a print speed of 90 mm / s, and a layer thickness of 100 μm. It was then co-laminated with a PVB film with a plasticizer content of 27.5% and a refractive index of 1,47979. This laminate appears transparent, but suppresses the aforementioned optical properties.

[0087] In another example, a pattern was punched out of a PVB film having a thickness of 100 μm and a refractive index of 1,48995 and co-laminated with a PVB film having a plasticizer content of 27.5% and a refractive index of 1,47979.

[0088] In a third example, white, pigmented Polysmooth PVB filament from Polymaker was 3D printed to create a structure that was flat on one side and exhibited varying thicknesses on the other. A film was 3D printed with clear Polysmooth PVB filament to match the height difference so that when bonded, both outer surfaces of the film appeared flat, enabling lamination with flat glass.

Claims

1. Laminated glass comprising two sheets of glass bonded together by an adhesive film, the adhesive film comprising: at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB; and at least one film A comprising polyvinyl acetal PA and optionally at least one plasticizer WA, characterized in that the refractive indices of film A and film B differ by at least 0.0002 and wherein the thickness of film A is from 5 μm to 20 μm and the thickness ratio of film A to film B in the starting state before lamination is less than 0.2, and film A comprises alkali metal ions and / or alkaline earth metal ions to adjust the level of adhesion to the glass, wherein, in order to avoid fogging, the amount of chloride ions and / or nitrate ions and / or sulfate ions in film A can be reduced.

2. The laminated glass according to claim 1, characterized in that: The laminated glass has two surface regions and at least three edge regions, and wherein, when the laminated glass is illuminated from one of the edge regions or the surface regions, the refractive indices of film A and film B differ by at least 0.0002.

3. The laminated glass according to any one of claims 1 to 2, characterized in that: At least one of the edge region or the surface region is provided with lighting or daylight.

4. The laminated glass according to any one of claims 1 to 3, characterized in that: Prior to bonding the two glass sheets, the amount of plasticizer WA in film A is less than 45% by weight, and the amount of plasticizer WB in film B is less than 45% by weight.

5. The laminated glass according to any one of claims 1 to 4, characterized in that: The film A is provided by printing a melt comprising polyvinyl acetal PA and optionally at least one plasticizer WA onto or into the film B.

6. The laminated glass according to any one of claims 1 to 5, characterized in that: Film A is provided by combining film B with a cut-out or punched pattern of film A comprising polyvinyl acetal PA and optionally at least one plasticizer WA.

7. The laminated glass according to claim 1, characterized in that: The film A is sandwiched between two films B comprising identical or different polyvinyl acetals PB and at least one plasticizer WB.

8. The laminated glass according to claim 1, characterized in that: Film A includes an inorganic filler, a pigment or a dye.

9. The laminated glass according to claim 1, characterized in that: Film B includes an inorganic filler, a pigment or a dye.

10. The laminated glass according to any one of claims 1 to 7, characterized in that: The thickness ratio of film A to film B is between 0.002 and 1, preferably between 0.002 and 0.

2.

11. The laminated glass according to any one of claims 1 to 8, characterized in that: Film B comprises at least two layers, wherein the amount of plasticizer WB in the layers differs by at least 2% by weight.

12. The laminated glass according to any one of claims 1 to 9, characterized in that: Film B has a wedge-shaped thickness profile.

13. A process for manufacturing laminated glass by bonding two sheets of glass with an adhesive film, the adhesive film comprising: at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB; and at least one film A comprising polyvinyl acetal PA and optionally at least one plasticizer WA, wherein the refractive index of film A or film B differs by at least 0.0002 by printing a melt comprising polyvinyl acetal PA and optionally at least one plasticizer WA on or into film B, and wherein the thickness of film A is from 5 μm to 20 μm and the thickness ratio of film A to film B in the starting state before lamination is less than 0.2, and film A comprises alkali metal ions and / or alkaline earth metal ions to adjust the level of adhesion to glass, wherein, in order to avoid hazing, the amount of chloride ions and / or nitrate ions and / or sulfate ions in film A can be reduced.