Anti-ultraviolet polypropylene synthetic paper and preparation method thereof
By introducing modified anti-ultraviolet agent and calcium carbonate into polypropylene synthetic paper, combined with extrusion and stretching processes, the problem of easy damage and insufficient anti-aging performance of polypropylene synthetic paper outdoors is solved, and high mechanical strength and resistance are achieved Improved combustion performance.
Patent Information
- Application Number
- CN202411454440.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-10-17
AI Technical Summary
Existing polypropylene synthetic paper is prone to breaking and yellowing when used outdoors, and its anti-ultraviolet aging and flame retardant properties are poor.
UV-resistant polypropylene synthetic paper consisting of an outer surface layer, an intermediate layer and an inner surface layer. The outer surface layer and the inner surface layer are composed of polypropylene, polypropylene carbonate, modified anti-ultraviolet agent and calcium carbonate. The intermediate layer is also composed of The anti-ultraviolet agent is prepared by reacting under the protection of dibenzoyl peroxide by DMF media, which increases the molecular weight and light stability of the anti-ultraviolet agent, and is prepared by extrusion, stretching, corona and other processes.
The UV aging resistance and flame retardant properties of polypropylene synthetic paper are improved, and excellent mechanical properties and flame retardant grade are maintained. After aging, it still has high mechanical strength and V-0 flame retardant grade.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of synthetic paper, and in particular to an anti-ultraviolet polypropylene synthetic paper and a preparation method thereof. Background Art
[0002] Polypropylene synthetic paper has many advantages, such as low carbon and environmental protection, low specific gravity, high strength, good weather resistance, good tear resistance, soft texture, excellent printing performance and durability. Polypropylene synthetic paper has been widely used in high-quality printing, high-end packaging and special uses because it has the characteristics of both plastic and paper. With the increase in the application scenarios of polypropylene synthetic paper, such as easy breakage after long-term outdoor exposure, yellowing and fading, more requirements are put forward for polypropylene synthetic paper, such as anti-ultraviolet aging performance when used outdoors.
[0003] A Chinese invention patent with publication number CN104943308A discloses a polypropylene synthetic paper and a production method thereof. The polypropylene synthetic paper includes an outer layer, an intermediate layer and an inner layer. The outer layer is mainly prepared from titanium dioxide, calcium carbonate and a modified polypropylene copolymer, the intermediate layer is mainly prepared from polypropylene, and the inner layer is mainly prepared from titanium dioxide, calcium carbonate and a modified polypropylene copolymer. The paper has excellent mechanical properties, but poor UV resistance, anti-aging and flame retardancy. Summary of the invention
[0004] In view of the shortcomings of the prior art, an object of the present invention is to provide an anti-ultraviolet polypropylene synthetic paper and a preparation method thereof.
[0005] To achieve the above object, the present invention is implemented through the following technical solutions: An anti-ultraviolet polypropylene synthetic paper, consisting of an outer layer, an intermediate layer and an inner layer, wherein the outer layer is composed of the following raw materials in parts by weight: 40-50 parts of polypropylene, 20-30 parts of polypropylene carbonate, 2-4 parts of modified anti-ultraviolet agent, and 1-2 parts of calcium carbonate; The middle layer is composed of the following raw materials in parts by weight: 20-30 parts of polypropylene, 30-40 parts of polypropylene carbonate, 2-4 parts of modified anti-ultraviolet agent, and 1-2 parts of calcium carbonate; The raw materials and the number of portions of the inner surface layer are the same as those of the outer surface layer; The modified UV-resistant agent is prepared by the following method: DMF was added to the reaction bottle, and the temperature was raised to 75-95°C with stirring, and 2-hydroxy-4-acrylate-benzophenone, (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and dibenzoyl peroxide were added in sequence, and the reaction was carried out under nitrogen protection for 8-10 hours to obtain a reddish brown solution, which was rotary evaporated and vacuum dried at 50-60°C to obtain a modified UV inhibitor. The reaction equation is shown as follows:
[0006] The mass ratio of DMF, dibenzoyl peroxide, (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and 2-hydroxy-4-acrylate-benzophenone is (20-30):(0.4-0.8):(2-3):5.
[0007] A method for preparing UV-resistant polypropylene synthetic paper comprises the following steps: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.
[0008] Due to the adoption of the above technical solution, the beneficial effects of the present invention include: (1) The present invention uses (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide and 2-hydroxy-4-acrylate-benzophenone to prepare a modified UV-resistant agent for polypropylene synthetic paper under the action of an initiator dibenzoyl peroxide.
[0009] (2) The 2-hydroxy-4-acrylate-benzophenone used in the modified UV inhibitor prepared by the present invention has a hydroxyl group and can be chemically bonded to the polymer during the manufacturing process of synthetic paper, so that it has an inherent "permanent" UV absorption group. However, due to its small molecular weight, it is not resistant to migration. By reacting with (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, the molecular weight of the UV inhibitor is increased, so that it has both excellent light stabilization effect and the advantages of migration resistance and extraction resistance, thereby improving the ability of synthetic paper to resist UV aging.
[0010] (3) The (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide used in the present invention can capture free radicals and play a role in gas phase flame retardancy, while promoting the formation of a carbon layer, thereby improving the flame retardancy of synthetic paper. DETAILED DESCRIPTION
[0011] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.
[0012] Example 1 Preparation of modified UV-resistant agent: Add 2000g DMF to the reaction bottle, stir and heat to 75°C, add 500g 2-hydroxy-4-acrylate-benzophenone, 200g (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and 40g dibenzoyl peroxide in sequence, react for 10h under nitrogen protection to obtain a reddish brown solution, rotary evaporate, and vacuum dry at 50°C for 8h to obtain a modified UV inhibitor.
[0013] Example 2 Preparation of modified UV-resistant agent: Add 2500g DMF to the reaction bottle, stir and heat to 85°C, add 500g 2-hydroxy-4-acrylate-benzophenone, 250g (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, 60g dibenzoyl peroxide in sequence, react under nitrogen protection for 9h to obtain a reddish brown solution, rotary evaporate, vacuum dry at 55°C for 8h to obtain a modified UV inhibitor. Its H NMR spectrum data are as follows: 1 H NMR (500 MHz, Chloroform- d ) δ12.21(s, 1H), 8.18 (ddd, J= 12.9,7.4, 1.3 Hz, 2H), 7.95 – 7.88 (m, 1H), 7.80 – 7.72 (m, 3H), 7.71 (d, J = 8.4Hz, 1H), 7.65 – 7.57 (m, 2H), 7.55 – 7.46 (m, 4H), 7.49 – 7.40 (m, 2H), 7.21 – 7.15 (m, 2H), 6.81 – 6.75 (m, 2H), 6.70 (dd, J = 8.3, 2.3 Hz, 1H), 6.45 (d, J = 2.3 Hz, 1H), 4.34 (dd, J = 11.8, 5.7 Hz, 1H), 4.23 (dd, J = 12.1, 5.7 Hz,1H), 4.12 – 3.94 (m, 3H), 3.78 – 3.71 (m, 1H), 3.52 (d, J = 6.3 Hz, 1H), 2.61– 2.46 (m, 2H), 2.43 (dt, J = 14.5, 8.6 Hz, 1H), 2.26 (dq, J = 13.4, 8.2 Hz,1H).
[0014] Example 3 Preparation of modified UV-resistant agent: Add 3000g of DMF to the reaction bottle, stir and heat to 95°C, add 500g of 2-hydroxy-4-acrylate-benzophenone, 300g of (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and 80g of dibenzoyl peroxide in sequence, react under nitrogen protection for 8h to obtain a reddish brown solution, rotary evaporate, and vacuum dry at 60°C for 6h to obtain a modified UV inhibitor.
[0015] Example 4
[0016] A UV-resistant polypropylene synthetic paper has a thickness of 0.20 mm, an outer layer and an inner layer both having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer comprises 4000 g of polypropylene, 2000 g of polypropylene carbonate, 200 g of a modified UV-resistant agent (prepared in Example 1), and 100 g of calcium carbonate; the middle layer comprises 2000 g of polypropylene, 3000 g of polypropylene carbonate, 200 g of a modified UV-resistant agent (prepared in Example 1), and 100 g of calcium carbonate; and the inner layer has the same raw materials and proportions as the outer layer.
[0017] Example 5
[0018] A UV-resistant polypropylene synthetic paper has a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer is made of the following raw materials: 4500 g of polypropylene, 2500 g of polypropylene carbonate, 300 g of a modified UV-resistant agent (prepared in Example 2), and 150 g of calcium carbonate; the middle layer is made of the following raw materials: 2500 g of polypropylene, 3500 g of polypropylene carbonate, 300 g of a modified UV-resistant agent (prepared in Example 2), and 150 g of calcium carbonate; and the inner layer has the same raw materials and proportions as the outer layer.
[0019] Example 6
[0020] A UV-resistant polypropylene synthetic paper has a thickness of 0.20 mm, an outer layer and an inner layer both having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer is made of the following raw materials: 5000 g of polypropylene, 3000 g of polypropylene carbonate, 400 g of a modified UV-resistant agent (prepared in Example 3), and 200 g of calcium carbonate; the middle layer is made of the following raw materials: 3000 g of polypropylene, 4000 g of polypropylene carbonate, 400 g of a modified UV-resistant agent (prepared in Example 3), and 200 g of calcium carbonate; and the raw materials and proportions of the inner layer are the same as those of the outer layer.
[0021] Comparative Example 1 A UV-resistant polypropylene synthetic paper is basically the same as Example 5, except that no modified UV-resistant agent is added to the outer layer and the inner layer.
[0022] Comparative Example 2 A UV-resistant polypropylene synthetic paper is basically the same as Example 5, except that the modified UV-resistant agent added to the outer layer and the inner layer is replaced by an equal weight of 2-hydroxy-4-acrylate-benzophenone.
[0023] Comparative Example 3 A UV-resistant polypropylene synthetic paper is basically the same as Example 5, except that the modified UV-resistant agent added to the outer layer and the inner layer is replaced by an equal weight of (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide.
[0024] Comparative Example 4 A UV-resistant polypropylene synthetic paper is basically the same as Example 5, except that the modified UV-resistant agent added to the outer layer and the inner layer is replaced by 200g of 2-hydroxy-4-acrylate-benzophenone and 100g of (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide.
[0025] Comparative Example 5 A UV-resistant polypropylene synthetic paper, wherein the raw materials and proportions of the outer layer, the middle layer and the inner layer are the raw materials and proportions of Example 1 of the Chinese invention patent with publication number CN104943308A.
[0026] The UV-resistant polypropylene synthetic paper of Examples 4-6 and Comparative Examples 1-5 was prepared by the following process: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.
[0027] The polypropylene used in the examples and comparative examples of the present application is CJS-700 homopolymer polypropylene produced by Sinopec, and the weight average molecular weight of polypropylene carbonate is 1.3×10 5 The brand of calcium carbonate is Qiagen KJ-106.
[0028] The polypropylene synthetic papers prepared in Examples 4-6 and Comparative Examples 1-5 were subjected to UV aging tests, and the test method was carried out according to the method of GB / T 16422.3-2014 "Plastics Laboratory Light Source Exposure Test Method".
[0029] The polypropylene synthetic paper prepared in Examples 4-6, Comparative Examples 1-5, and the aged polypropylene synthetic paper were subjected to tensile strength tests according to the method of GB13022-91; the test results of Examples 4-6 of the present application are shown in Table 1.
[0030] The polypropylene synthetic paper prepared in Examples 4-6 and Comparative Examples 1-5 and the aged synthetic paper were subjected to a vertical burning (UL-94) test. According to the ASTM D3801 standard, the vertical burning grade of the samples was evaluated using a CZF-3 instrument. The sample size was 130×13×3.2 mm 3 (Its thickness is achieved by stacking layers of synthetic paper). The test results are shown in Table 1.
[0031] Table 1
[0032] It can be seen from Examples 4, 5 and 6 in Table 1 that the polypropylene synthetic paper prepared by the present invention has transverse and longitudinal mechanical strengths greater than 120 MPa and 75 MPa, respectively, and the transverse and longitudinal mechanical strengths after aging are greater than 110 MPa and 65 MPa, respectively, and has excellent transverse and longitudinal mechanical properties, and the flame retardant grade remains at V-0 level after aging.
[0033] Comparative Example 1 is a comparative example without adding an anti-ultraviolet agent. After aging, its transverse mechanical strength is lower than 81 MPa, its longitudinal tensile strength is 49 MPa, and its flammability rating (UL-94) is V-2.
[0034] Comparative Example 2 is different from Example 5 in that the modified UV inhibitor is replaced with 2-hydroxy-4-acrylate-benzophenone. After aging, the transverse mechanical strength is 101 MPa, the longitudinal tensile strength is 60 MPa, and the flammability rating (UL-94) is V-2.
[0035] Comparative Example 3 is different from Example 5, and the difference is that the modified anti-ultraviolet agent is replaced by 2,4-dihydroxybenzophenone and (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide. It can be seen from the data in Table 1 that the mechanical properties before aging are basically similar to those of Example 5, but after aging, the transverse tensile strength is 83 MPa, the longitudinal tensile strength is 50 MPa, the mechanical strength loss is serious, and the flammability rating (UL-94) is V-0.
[0036] Comparative Example 4 is different from Example 5, in that the modified UV inhibitor is replaced with (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and after aging, the transverse mechanical strength is 96 MPa, the longitudinal tensile strength is 57 MPa, and the flammability rating (UL-94) is V-1.
[0037] Comparative Example 5 is a synthetic paper prepared using the raw materials and proportions in Example 1 of the Chinese invention patent with publication number CN104943308A. After aging, its transverse tensile strength is 88 MPa, its longitudinal tensile strength is less than 49 MPa, and its flammability rating (UL-94) is V-2.
[0038] In summary, it can be seen from the data of the comparative examples and embodiments in Table 1 that the UV-resistant polypropylene synthetic paper prepared by the present invention has excellent transverse and longitudinal mechanical properties, still maintains relatively good mechanical properties after aging, and has excellent flame retardant properties.
[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A UV-resistant polypropylene synthetic paper, comprising an outer layer, an intermediate layer and an inner layer, characterized in that: The outer layer is composed of the following raw materials in parts by weight: 40-50 parts of polypropylene, 20-30 parts of polypropylene carbonate, 2-4 parts of modified anti-ultraviolet agent, and 1-2 parts of calcium carbonate; The middle layer is composed of the following raw materials in parts by weight: 20-30 parts of polypropylene, 30-40 parts of polypropylene carbonate, 2-4 parts of modified anti-ultraviolet agent, and 1-2 parts of calcium carbonate; The raw materials and the number of portions of the inner surface layer are the same as those of the outer surface layer; The modified UV-resistant agent is prepared by the following method: Add DMF to the reaction bottle, stir and heat to 75-95°C, add 2-hydroxy-4-acrylate-benzophenone, (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide and dibenzoyl peroxide in sequence, react for 8-10 hours under nitrogen protection to obtain a reddish brown solution, rotary evaporate, and vacuum dry at 50-60°C to obtain a modified UV inhibitor.
2. The UV-resistant polypropylene synthetic paper according to claim 1, characterized in that: The mass ratio of DMF, dibenzoyl peroxide, (6S)-6-(hydroxy(4-hydroxyphenyl)methyl)dibenzo[c,e][1,2]phosphazene 6-oxide, and 2-hydroxy-4-acrylate-benzophenone is (20-30):(0.4-0.8):(2-3):
5.
3. A method for preparing the UV-resistant polypropylene synthetic paper according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.
Citation Information
Patent Citations
Polypropylene carbonate modified composite material and preparation method thereof
CN104017348A
Flame-retardant modifier, preparation and method for preparing flame-retardant material through ultraviolet light initiation
CN116145415A
Anti-aging PVC (polyvinyl chloride) material and synthesis process
CN116589803A
Degradable polypropylene synthetic paper and preparation method thereof
CN117734275A
Preparation method of uvioresistant thermoplastic polyurethane elastomer
CN118755252A
Cited By
PP / PE biaxially oriented synthetic paper and preparation method thereof
CN119159891A