High-purity indium telluride and preparation method thereof

Through the three-stage heating method, the problems of high loss and low purity in the preparation process of indium telluride were solved, and the preparation of high-purity indium telluride was achieved, which reduced the loss of telluride and ensured the thoroughness of the reaction and the uniformity of the system.

CN118978129APending Publication Date: 2024-11-19XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411295109.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-15
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, there is a problem that the loss is high during the preparation process of indium telluride and the purity is difficult to improve.

Method used

The three-stage heating method is adopted, first the solid solution reaction is performed above the melting point temperature of indium, then the liquid-liquid reaction is performed above the melting point temperature of tellurium, and finally the reaction is completed above the melting point of indium tellurium, by adjusting the molar ratio of tellurium and indium Heating speed reduces the loss of tellurium and improves purity.

Benefits of technology

It effectively reduces the loss of tellurium, improves the purity of indium telluride, and ensures the thoroughness of the reaction and the uniformity of the system through phased heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045720830000081
    Figure BDA0005045720830000081
Patent Text Reader

Abstract

The invention belongs to the technical field of new materials, and discloses a preparation method of high-purity indium telluride, which comprises the following steps: step 1, mixing tellurium and indium according to a molar ratio of (1.05-1.1): 1, heating to a first temperature, and keeping the temperature; 2, heating a product obtained in the step 1 to a second temperature, and keeping the temperature; 3, heating a product obtained in the step 2 to a third temperature, and preserving heat; step 4, cooling to obtain high-purity indium telluride; the first temperature is higher than the melting point of indium and lower than the melting point of tellurium; the second temperature is higher than the melting point of tellurium and lower than the melting point of indium telluride; the third temperature is higher than the melting point of indium telluride. According to the method, the loss of tellurium can be minimized, and meanwhile, the purity of indium telluride is improved. Meanwhile, the invention further provides the high-purity indium telluride prepared on the basis of the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to high-purity indium telluride and a preparation method thereof. Background Art

[0002] Indium telluride, with the chemical formula InTe, belongs to the III-V group of compound materials with a cubic lattice structure. Due to its special physical and chemical properties, it is widely used in electronics, optoelectronics, infrared detectors, solar cells and other fields. Its crystal structure is compact and not prone to chemical reactions. Therefore, indium telluride has good chemical stability and corrosion resistance. It is also hard and can be used to manufacture wear-resistant and high-temperature resistant devices.

[0003] The preparation method of indium telluride is generally to heat the mixture of tellurium and indium to a temperature above the melting point of tellurium to react so that the reaction raw materials react in liquid-liquid contact. For example, CN111115590A discloses a two-dimensional indium telluride nanosheet and a polarized light detector prepared therefrom, which is prepared by this method, and the molar ratio of indium powder to tellurium powder is 1: (2-3). The reason why such a large amount is used is that the vapor pressure of tellurium powder is relatively high and it is easy to be carried away under the protection of inert gas, so an excess of tellurium powder is used to balance the material carried away by the protective gas.

[0004] The technical problem solved in this case is how to reduce the loss in the preparation process of indium telluride and how to improve the purity of indium telluride. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing high-purity indium telluride, which can minimize the loss of tellurium and improve the purity of indium telluride.

[0006] At the same time, the present invention also provides high-purity indium telluride prepared based on the method.

[0007] To achieve the above objectives, this application discloses:

[0008] A method for preparing high-purity indium telluride comprises the following steps:

[0009] Step 1: mixing tellurium and indium in a molar ratio of 1.05 to 1.1:1, heating to a first temperature, and keeping the temperature;

[0010] Step 2: heating the product of step 1 to a second temperature and keeping the temperature;

[0011] Step 3: heating the product of step 2 to a third temperature and keeping the temperature;

[0012] Step 4: Cooling to obtain high-purity indium telluride;

[0013] The first temperature is higher than the melting point of indium and lower than the melting point of tellurium;

[0014] The second temperature is higher than the melting point of tellurium and lower than the melting point of indium telluride;

[0015] The third temperature is higher than the melting point of indium telluride.

[0016] The design key points of the present invention are:

[0017] 1. Through the solid solution reaction of tellurium and indium in step 1, most of the indium telluride is generated; however, in this process, there will be a situation where indium telluride wraps around tellurium, resulting in the inability to further proceed with the solid solution reaction;

[0018] 2. Through the liquid-liquid reaction in step 2, most of the indium telluride is generated; and in this process, the content of elemental tellurium is already very small, so less tellurium vapor will be taken away. According to the molar ratio of 1.05 to 1.1:1, the excess elemental tellurium can make up for this part of the carrier gas loss;

[0019] 3. Through the temperature increase reaction in step 3, the complete generation of indium telluride can be achieved.

[0020] Through the above reaction, high-purity synthesis of indium telluride can be achieved while reducing the loss of tellurium.

[0021] In the above preparation method, in step 1, tellurium exists in the form of tellurium powder; and indium exists in the form of indium blocks.

[0022] Indium has a low melting point and is difficult to prepare indium powder, so indium is present in the form of indium blocks in the present invention, which can reduce the difficulty of production.

[0023] In the above preparation method, in step 1, indium is placed below tellurium.

[0024] During the heating process, indium will melt first, and the tellurium filled in the gaps of the indium block will first enter the indium solution for a solid solution reaction, and then the remaining tellurium powder floating on the upper surface will continue to enter the indium solution for a solid solution reaction, which can effectively reduce the degree of indium telluride wrapping the tellurium powder; if indium is mixed with tellurium powder in a powder state, after the indium becomes liquid, due to the presence of a large amount of tellurium powder and simultaneous solid solution, the tellurium powder will fully contact the tellurium powder to form a state where indium telluride wraps the tellurium powder, hindering the further progress of the reaction; therefore, by placing the indium block below the tellurium, the degree of high solid solution reaction can be promoted.

[0025] In the above preparation method, the first temperature is 200-300°C; the second temperature is 500-600°C; and the third temperature is 750-850°C.

[0026] In the above preparation method, the insulation time of step 1 is 120 to 180 min; the insulation time of step 2 is 60 to 120 min; and the insulation time of step 3 is 120 to 180 min.

[0027] In the above preparation method, in step 1, the heating rate from room temperature to the first temperature is 5 to 15°C / min; the heating rate in step 2 is 5 to 15°C / min; and the heating rate in step 3 is 5 to 10°C / min.

[0028] In the above preparation method, in step 1 to step 4, flowing inert gas is used as protective gas; the flow rate of the protective gas is 3 to 5 L / min.

[0029] In the above preparation method, steps 1 to 4 are carried out in a graphite boat; the graphite boat is sent into a tubular heating furnace for reaction; and protective gas is introduced into the tubular heating furnace.

[0030] At the same time, the present invention also discloses a high-purity indium telluride, which is prepared by any of the above-mentioned preparation methods.

[0031] This application has at least the following beneficial effects:

[0032] The present invention divides the temperature rise of the reaction process into three stages, namely the first temperature, the second temperature and the third temperature. Most of the reactions are carried out in the first stage, that is, a solid solution reaction is carried out above the melting point of indium. In this step, there may be a situation where indium telluride wraps the tellurium powder, resulting in the inability to carry out the reaction thoroughly. Therefore, the temperature is raised to the second temperature. At this stage, the tellurium content is not much. Even if it forms steam, it will not be taken away too much by the carrier gas. After this stage, the tellurium content is already very small. Finally, the temperature is raised to the third temperature. At this stage, it is ensured that the reaction is carried out thoroughly. After the above-mentioned staged temperature rise, the loss of tellurium can be minimized and the purity of indium telluride can be improved. DETAILED DESCRIPTION

[0033] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0034] Example 1

[0035] A method for preparing high-purity indium telluride comprises the following steps:

[0036] Step 1. Put tellurium powder and indium block in a molar ratio of 1.1:1 into a graphite boat, with the indium block on the bottom layer and the tellurium powder on the top layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of the tellurium powder is ≤150um; part of the tellurium powder will fill the gaps in the indium block, and part of the tellurium powder will cover the surface of the indium block.

[0037] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 15 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0038] Step 3. In the first insulation stage, the temperature is heated from room temperature to 200°C at 10°C / min for 180 minutes. In the second insulation stage, the temperature is heated to 500°C at 15°C / min for 120 minutes. Then, in the third insulation stage, the temperature is heated to 800°C at 8°C / min for 120 minutes. The temperature is then lowered along with the furnace to obtain high-purity indium telluride.

[0039] Example 2

[0040] A method for preparing high-purity indium telluride comprises the following steps:

[0041] Step 1. Put tellurium powder and indium block in a molar ratio of 1.05:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0042] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 10 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 3 L / min.

[0043] Step 3. In the first insulation stage, the temperature is heated from room temperature to 250°C at 15°C / min for 160 minutes. In the second insulation stage, the temperature is heated to 600°C at 5°C / min for 60 minutes. Then, in the third insulation stage, the temperature is heated to 850°C at 10°C / min for 120 minutes. The temperature is lowered along with the furnace to obtain high-purity indium telluride.

[0044] Example 3

[0045] A method for preparing high-purity indium telluride comprises the following steps:

[0046] Step 1. Put tellurium powder and indium block in a molar ratio of 1.1:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0047] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 12 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 4 L / min.

[0048] Step 3. In the first insulation stage, the temperature is heated from room temperature to 300°C at 10°C / min for 120 minutes. In the second insulation stage, the temperature is heated to 550°C at 10°C / min for 100 minutes. Then, in the third insulation stage, the temperature is heated to 750°C at 5°C / min for 180 minutes. The temperature is lowered along with the furnace to obtain high-purity indium telluride.

[0049] Example 4

[0050] A method for preparing high-purity indium telluride comprises the following steps:

[0051] Step 1. Put tellurium powder and indium block in a molar ratio of 1.08:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0052] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 12 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0053] Step 3. In the first insulation stage, the temperature is heated from room temperature to 220°C at 12°C / min and kept for 160 minutes. In the second insulation stage, the temperature is heated to 520°C at 12°C / min and kept for 110 minutes. Then, in the third insulation stage, the temperature is heated to 770°C at 8°C / min and kept for 160 minutes. The temperature is lowered along with the furnace to obtain high-purity indium telluride.

[0054] Example 5

[0055] A method for preparing high-purity indium telluride comprises the following steps:

[0056] Step 1. Put tellurium powder and indium block into a graphite boat at a molar ratio of 1.06:1, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0057] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 12 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0058] Step 3. In the first insulation stage, the temperature is heated from room temperature to 280°C at 8°C / min and kept for 130 minutes. In the second insulation stage, the temperature is heated to 580°C at 8°C / min and kept for 80 minutes. Then, in the third insulation stage, the temperature is heated to 830°C at 10°C / min and kept for 140 minutes. The temperature is lowered along with the furnace to obtain high-purity indium telluride.

[0059] Comparative Example 1

[0060] A method for preparing indium telluride comprises the following steps:

[0061] Step 1. Put tellurium powder and indium block in a molar ratio of 1.1:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0062] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 15 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0063] Step 3. Heat from room temperature to 550°C at 15°C / min and keep at this temperature for 360 min, then cool down the furnace to obtain indium telluride.

[0064] Comparative Example 2

[0065] A method for preparing indium telluride comprises the following steps:

[0066] Step 1. Put tellurium powder and indium block in a molar ratio of 1.1:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0067] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 15 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0068] Step 3. Heat from room temperature to 800°C at 15°C / min and keep at this temperature for 360 min, then cool down the furnace to obtain indium telluride.

[0069] Comparative Example 3

[0070] A method for preparing indium telluride comprises the following steps:

[0071] Step 1. Put tellurium powder and indium block in a molar ratio of 1.1:1 into a graphite boat, with indium block placed in the lower layer and tellurium powder in the upper layer. The indium block is a small block with a diameter of no more than 5 cm; the average particle size of tellurium powder is ≤150um;

[0072] Step 2. The above materials are loaded into a horizontal tubular heating furnace and an inert gas is introduced at a gas flow rate of 15 L / min. After the inert gas is introduced for 30 minutes, heating is started and the nitrogen flow rate is changed to 5 L / min.

[0073] Step 3. In the first insulation stage, the temperature is heated from room temperature to 500°C at 15°C / min for 240 minutes, and then in the second insulation stage, the temperature is heated to 800°C at 8°C / min for 120 minutes, and the temperature is lowered along with the furnace to obtain high-purity indium telluride.

[0074] Performance Testing

[0075] Detect the concentration of free tellurium and free indium in the product by DSC

[0076] The test results refer to Table 1;

[0077] Table 1 Test results

[0078]

[0079] Result analysis:

[0080] 1. It can be seen from the cases of Examples 1 to 5 that the purity of the product can be significantly improved by increasing the temperature in stages;

[0081] When tellurium and indium are blended at a molar ratio of 1.05 to 1.1:1, in step 1, most of the indium telluride has been generated, and at this temperature, tellurium will not volatilize, and the carrier gas will not cause telluride to be lost. Although indium has a low melting point, it is not easy to form vapor. Therefore, in step 1, the loss of the element is small; in step 2, the residual tellurium and indium further melt and react. Under this temperature condition, tellurium begins to melt. Since the amount of tellurium and indium is already small, the reaction can be fully and quickly completed. In this process, there will be a problem of the carrier gas taking away the tellurium vapor, but since the tellurium is excessive, the excess tellurium can completely make up for the loss of tellurium vapor. In step 3, the temperature is raised to a temperature higher than the melting point of indium telluride, so that the system can form a uniform phase. This step is conducive to the uniformity of the system, improves the purity of the product, and completely evaporates the excess tellurium.

[0082] Therefore, this case is divided into three steps of heating, which can effectively improve product purity and reduce energy consumption.

[0083] 2. As can be seen from Comparative Example 1, in Comparative Example 1, when the temperature remains higher than the melting temperature of indium and lower than the melting temperature of indium telluride, the reaction cannot be carried out thoroughly. The possible reasons are as follows:

[0084] The temperature stays at the tellurium melting point for too long and there is no low-temperature melting process, resulting in tellurium being in a single substance state during the constant temperature process. It is excessively carried away by the carrier gas, resulting in a lot of indium residue. Without going through the temperature range of 750-850°C, the system may be uneven, resulting in excessive indium and tellurium in some areas.

[0085] 3. It can be seen from Comparative Example 2 that when the temperature rises to the melting temperature of indium telluride, although more tellurium is carried away by the carrier gas, the uniformity of the system becomes higher, which will result in indium not reacting completely. Except for the part of tellurium carried away by the carrier gas, the rest has reacted fully.

[0086] 4. It can be seen from Comparative Example 3 that when there are second-stage heat preservation and third-stage heat preservation, the problem of excessive indium residue can be effectively solved. The reaction is achieved through the second-stage heat preservation, and the uniformity of the system is achieved through the third-stage heat preservation.

[0087] Based on the above experiments, the method of the present invention can effectively improve the purity of the product through the three-stage heat preservation operation.

[0088] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing high-purity indium telluride, characterized in that: The steps include: Step 1: mixing tellurium and indium in a molar ratio of 1.05 to 1.1:1, heating to a first temperature, and keeping the temperature; Step 2: heating the product of step 1 to a second temperature and keeping the temperature; Step 3: heating the product of step 2 to a third temperature and keeping the temperature; Step 4: Cooling to obtain high-purity indium telluride; The first temperature is higher than the melting point of indium and lower than the melting point of tellurium; The second temperature is higher than the melting point of tellurium and lower than the melting point of indium telluride; The third temperature is higher than the melting point of indium telluride.

2. The preparation method according to claim 1, characterized in that: In the step 1, tellurium exists in the form of tellurium powder; and indium exists in the form of indium blocks.

3. The preparation method according to claim 1, characterized in that: In step 1, indium is placed below tellurium.

4. The preparation method according to claim 1, characterized in that: The first temperature is 200-300°C; the second temperature is 500-600°C; and the third temperature is 750-850°C.

5. The preparation method according to claim 1, characterized in that: The heat preservation time of step 1 is 120 to 180 minutes; the heat preservation time of step 2 is 60 to 120 minutes; and the heat preservation time of step 3 is 120 to 180 minutes.

6. The preparation method according to claim 1, characterized in that: In the step 1, the heating rate from room temperature to the first temperature is 5 to 15°C / min; the heating rate in the step 2 is 5 to 15°C / min; and the heating rate in the step 3 is 5 to 10°C / min.

7. The preparation method according to claim 1, characterized in that: In step 1 to step 4, flowing inert gas is used as the protective gas; the flow rate of the protective gas is 3 to 5 L / min.

8. The preparation method according to claim 7, characterized in that: Steps 1 to 4 are carried out in a graphite boat; the graphite boat is sent into a tubular heating furnace for reaction; and protective gas is introduced into the tubular heating furnace.

9. A high-purity indium telluride, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of indium telluride nanometer lines

    CN108190847A

  • Preparation method of germanium telluride

    CN116715203A

  • Silver telluride and preparation method thereof

    CN117185264A

  • High-purity bismuth sulfide and preparation method thereof

    CN118145701A

  • Multi-nary group IB and via based semiconductor

    US20120168910A1