Carbon material with ultralow specific surface area, preparation method thereof and battery
By using thermoplastic phenolic resin and n-propanol to prepare ultra-low specific surface area carbon materials, the problems of large specific surface area and many mesoporous areas of carbon materials are solved, and the low electrolyte consumption, structural stability and high rate performance of the battery are achieved, and the battery is extended Lifespan and increase energy density.
Patent Information
- Application Number
- CN202410847226.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-06-27
AI Technical Summary
When used as the negative electrode of the battery, existing carbon materials have large specific surface area and large number of mesopories, resulting in large consumption of electrolytes and unstable structure, affecting the cycle life and energy density of the battery.
Thermoplastic phenolic resin and n-propanol are used as the closed-cell agent to prepare an ultra-low specific surface area carbon material through hydrothermal reaction and carbonization process to form a stable and uniform pore structure, which is used for the negative electrode of the battery to reduce the specific surface area and the number of mesoporous pores.
It significantly reduces electrolyte consumption, improves the structural stability and rate performance of the battery, extends the service life of the battery, and improves the energy density and first-time charge and discharge efficiency.
Smart Images

Figure CN118978140A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a negative electrode carbon material for a battery, and more particularly to an ultra-low specific surface area carbon material and a preparation method thereof, as well as a battery using the ultra-low specific surface area carbon material. Background Art
[0002] The internal structure of the battery is mainly composed of positive electrode, negative electrode, electrolyte and diaphragm. The stable development of the battery mainly depends on these four key systems, which together determine the quality of lithium-ion batteries.
[0003] The negative electrode material is the main body of lithium / sodium storage in lithium / sodium ion batteries. The function of the negative electrode active material is to reversibly absorb / release the lithium / sodium ions released by the positive electrode and output current through the external circuit. The negative electrode material of lithium / sodium ion batteries accounts for about 5-10% of the total cost of the battery, while the positive electrode material usually contains metal elements such as lithium, manganese, and cobalt, whose reserves are relatively limited and the market price is relatively high. More importantly, compared with the limited specific capacity of the positive electrode material, the negative electrode material is easier to achieve an increase in energy density.
[0004] The reaction ability of the battery's negative electrode material and lithium / sodium ions directly determines the battery's electrochemical performance. Currently, the negative electrode materials that are being studied more are mainly carbon materials such as graphite, silicon, and silicon-carbon alloy materials, among which the commercial negative electrode materials are mainly carbon materials such as graphite. Carbon negative electrode materials have a large specific surface area and more pores, which increases their SEI film, consumes a large amount of electrolyte and active lithium, and the coulomb efficiency of the cycle gradually decreases, ultimately leading to battery capacity decay and limited cycle life. Summary of the invention
[0005] In view of this, the present invention provides an ultra-low specific surface area carbon material and a preparation method thereof. The present invention provides a battery comprising the aforementioned ultra-low specific surface area carbon material to solve the defects of existing carbon materials when used as battery negative electrodes, such as large specific surface area, large number of mesopores, large amount of electrolyte consumption when used as battery negative electrodes, and unstable structure.
[0006] In a first aspect, the present invention provides a method for preparing an ultra-low specific surface area carbon material, which comprises the following steps by weight:
[0007] Preparation of a closed-cell material: providing 10 to 50 parts of a thermoplastic phenolic resin and 10 parts of a closed-cell agent, mixing the thermoplastic phenolic resin and the closed-cell agent to obtain a mixed system, transferring the mixed system to 150 to 250° C. for hydrothermal reaction for 1 to 12 hours, and then transferring the mixed system to 80 to 150° C. for drying for 2 to 12 hours to obtain a closed-cell material;
[0008] Preparation of ultra-low specific surface area carbon material: placing the closed-cell material in an inert atmosphere at 1200-1700° C. for carbonization for 1-4 hours to obtain an ultra-low specific surface area carbon material;
[0009] The cell-blocking agent is n-propanol.
[0010] The preparation method of the ultra-low specific surface area carbon material of the present invention comprises the steps of preparing a closed-cell material and preparing an ultra-low specific surface area carbon material. In the step of preparing the closed-cell material, after the thermoplastic phenolic resin and the closed-cell agent react through addition, acetalization and the like, the surface of the thermoplastic phenolic resin reacts with the closed-cell agent and solidifies, and a smaller pore structure is formed on the surface of the thermoplastic phenolic resin to obtain a closed-cell material. In the step of preparing the ultra-low specific surface area carbon material, the closed-cell material is carbonized to obtain an ultra-low specific surface area carbon material. The preparation method of the ultra-low specific surface area carbon material of the present invention selects thermoplastic phenolic resin as a carbon source, because the thermoplastic phenolic resin still has a certain plasticity after solidification and can be processed and formed again. For example, the cured thermoplastic phenolic resin is first processed into a battery negative electrode shape, and then the processed thermoplastic phenolic resin is carbonized, and the ultra-low specific surface area carbon material after carbonization can be directly used as a battery negative electrode. By using thermoplastic phenolic resin, the ultra-low specific surface area carbon material prepared by the present application has better processing performance and can meet more complex shape and structural requirements. In contrast, ordinary phenolic resin is not plastic after curing and is not suitable for use in the preparation method of the ultra-low specific surface area carbon material of the present application.
[0011] The closed-cell agent used in the preparation method of the ultra-low specific surface area carbon material of the present invention is n-propanol. The molecular size and acetal reaction activity of n-propanol are moderate, and a relatively stable and uniform pore structure can be formed. The cured thermoplastic phenolic resin formed after the reaction has a relatively moderate specific surface area, and the surface pore structure is stable and uniform. The boiling point and volatility of n-propanol are moderate, and the loss is small during the curing process, and the integrity of the pore structure can be maintained. N-propanol is the best choice for participating in the curing of phenolic resin and forming a pore structure that is conducive to the storage of sodium ions. This method uses n-propanol as a raw material, and the raw material source is wide and the price is low. The preparation process includes addition reaction and acetal reaction, with few steps, simple operation, and easy large-scale production.
[0012] Preferably, in the step of preparing the closed-cell material, the amount of the thermoplastic phenolic resin is 15 to 25 parts, the mixed system is transferred to 160 to 200° C. for hydrothermal reaction for 2 to 8 hours, and then the mixed system is transferred to 100 to 130° C. for drying for 4 to 8 hours. The thermoplastic phenolic resin is cured by the hydrothermal addition and acetalization reaction between the thermoplastic phenolic resin and the closed-cell agent, and the cured thermoplastic phenolic resin can form a relatively stable and uniform pore structure to form closed cells.
[0013] Preferably, in the step of preparing the closed-cell material, the amount of the thermoplastic phenolic resin is 20 parts, the mixed system is transferred to 180° C. for hydrothermal reaction for 4 hours, and then the mixed system is transferred to 120° C. for vacuum drying for 6 hours. Appropriate hydrothermal reaction conditions allow the cured thermoplastic phenolic resin to have a better specific surface area and a pore structure of moderate size.
[0014] Preferably, in the step of preparing the ultra-low specific surface area carbon material, the closed-cell material is placed in a tubular furnace and the tubular furnace is filled with an inert gas, wherein the inert gas is nitrogen or argon, and then the tubular furnace is heated to 1200-1700°C and maintained for 1-4 hours to obtain the ultra-low specific surface area carbon material. The tubular furnace can provide stable high-temperature carbonization conditions, and the tubular furnace is first filled with an inert gas, and then the tubular furnace is heated to 1200-1700°C and maintained for 1-4 hours, which effectively prevents the closed-cell material from being oxidized at high temperatures.
[0015] More preferably, in the step of preparing the ultra-low specific surface area carbon material, the tube furnace is heated to 1500°C and maintained for 2 hours, the heating rate is 2°C / min, and the ultra-low specific surface area carbon material is obtained after natural cooling. Appropriate carbonization temperature and time are conducive to achieving complete carbonization of the phenolic resin material, while also not increasing the specific surface area of the carbon material due to high temperature expansion.
[0016] In a second aspect, the present invention further provides an ultra-low specific surface area carbon material, which is prepared by the preparation method of the ultra-low specific surface area carbon material described in any one of the first aspects.
[0017] The ultra-low specific surface area carbon material of the present invention has a low specific surface area and a closed surface mesoporous structure. When used as a negative electrode of a battery, it has the following advantages: (1) Low electrolyte consumption. The lower the specific surface area, the smaller the contact area between the material and the electrolyte, and the lower the electrolyte consumption. This is particularly important for batteries using liquid electrolytes, such as lithium-ion batteries and sodium batteries, because it can improve the energy density and cycle life of the battery.
[0018] (2) Good structural stability. The lower the specific surface area, the more stable the pore structure of the material is, and it is less likely to collapse or deform. This is very important for batteries that require long-term stable operation because it can improve the safety and reliability of the battery. (3) Excellent rate performance. Ultra-low specific surface area carbon materials have a fast lithium or sodium ion insertion / extraction rate and have excellent rate performance. This makes them very suitable for batteries that require high power applications such as electric vehicles and energy storage.
[0019] Preferably, the specific surface area of the ultra-low specific surface area carbon material is not greater than 12 m 2 / g. Specific surface area is less than 12m 2 / g, effectively reducing electrolyte consumption and improving battery energy density. The pore structure is stable and not prone to collapse or deformation, which improves the safety and reliability of the battery.
[0020] In a third aspect, the present invention further provides a battery, comprising the ultra-low specific surface area carbon material described in the second aspect.
[0021] The battery of the present invention uses an ultra-low specific surface area carbon material as the negative electrode, and has the advantages of low electrolyte consumption, good structural stability and excellent rate performance. The battery using the ultra-low specific surface area carbon material as the negative electrode shows very high first coulombic efficiency and specific capacity. It has excellent rate performance and is suitable for high-power applications. It has good cycle stability and a long service life. Specifically, as a negative electrode material for sodium ion batteries, the reversible specific capacity of the ultra-low specific surface area carbon material prepared by this method can reach more than 350mAh / g, and the first efficiency exceeds 90%.
[0022] Advantages of the present invention will be partially set forth in the following description, and partly will be obvious from the description, or may be learned through implementation of the embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the content of the present invention, it is described in detail below with reference to the accompanying drawings and specific embodiments.
[0024] Figure 1 This is a transmission electron microscope microscopic image of the ultra-low specific surface area carbon material prepared in Example 3;
[0025] Figure 2 This is a graph showing the nitrogen adsorption test results of the ultra-low specific surface area carbon material corresponding to Example 3;
[0026] Figure 3 This is the charge and discharge curve of the battery corresponding to Example 3. DETAILED DESCRIPTION
[0027] The following is a preferred embodiment of the present invention. It should be noted that a person skilled in the art may make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
[0028] The following describes in detail the method for preparing the ultra-low specific surface area carbon material of the present application and the advantages of the ultra-low specific surface area carbon material prepared therefrom through specific examples.
[0029] A method for preparing an ultra-low specific surface area carbon material comprises the steps of preparing a closed-cell material and preparing an ultra-low specific surface area carbon material.
[0030] Preparation of closed-cell material: providing thermoplastic phenolic resin and closed-cell agent, mixing the thermoplastic phenolic resin and closed-cell agent and then transferring them to a hydrothermal reactor lined with polytetrafluoroethylene, sealing the hydrothermal reactor and then placing the hydrothermal reactor at a certain temperature for reaction. After the reaction is completed, the reactants in the hydrothermal reactor are transferred to an oven and dried for a certain period of time to obtain a closed-cell material. See Table 1 for the amount of raw materials, hydrothermal reaction conditions, drying conditions, etc. in the specific embodiment.
[0031] Table 1 Condition parameters for the steps of preparing closed-cell materials
[0032]
[0033] Preparation of ultra-low specific surface area carbon material step: Place the closed-cell material obtained in the above step in a tubular furnace and fill the tubular furnace with inert gas, then heat the tubular furnace to the carbonization temperature and complete the carbonization step, and naturally cool under the inert gas atmosphere to obtain the ultra-low specific surface area carbon material. For the specific embodiment, the type of inert gas, carbonization temperature, carbonization time, heating rate, etc., see Table 2.
[0034] Table 2 Condition parameters for the steps of preparing ultra-low specific surface area carbon materials
[0035] Example Group Inert gas type Carbonization temperature(℃) Carbonization time (h) Heating rate (℃ / min) Example 1 Nitrogen 1600 2 2 Example 2 Argon 1400 3 2 Example 3 Nitrogen 1500 2 2 Example 4 Argon 1200 4 2 Example 5 Nitrogen 1700 1 2 Comparative Example 1 Nitrogen 1500 2 2 Comparative Example 2 Nitrogen 1500 2 2 Comparative Example 3 Nitrogen 1500 2 2
[0036] Effect Example 1: Transmission electron microscope microscopic detection of ultra-low specific surface area carbon materials
[0037] The ultra-low specific surface area carbon materials prepared in Examples 1-5 and Comparative Examples 1-3 were microscopically inspected using a transmission electron microscope to record the sealing conditions of the surface pores of the ultra-low specific surface area carbon materials. The results are shown in Table 3.
[0038] Table 3 Closure of pores on the surface of ultra-low specific surface area carbon materials
[0039] Example Group Hole situation Example 1 Closed holes and stable structure Example 2 Closed holes and stable structure Example 3 Closed holes and stable structure Example 4 Closed holes and stable structure Example 5 Closed holes and stable structure Comparative Example 1 Holes are closed, structures are unstable, and large amounts of collapse occur Comparative Example 2 Holes are closed and the structure is incomplete Comparative Example 3 Small holes, unstable structure, and massive collapse
[0040] Through transmission electron microscopic examination, it was found that the ultra-low specific surface area carbon materials prepared in Examples 1-5 all had closed pore structures on their surfaces, and the pore structures were stable and uniform. Figure 1 As shown, it is a transmission electron microscope microscopic detection image of the ultra-low specific surface area carbon material prepared in Example 3. This is related to the molecular size of n-propanol and the moderate activity of acetal reaction. The boiling point and volatility of n-propanol are moderate, and the loss is small during the curing process, and the integrity of the pore structure can be maintained. Therefore, n-propanol is the best choice for participating in the curing of phenolic resin and forming a pore structure that is conducive to the storage of sodium ions.
[0041] The ultra-low specific surface area carbon material prepared in Comparative Example 1 has closed pores on the surface, unstable structure, and a large number of pores collapsed. Since methanol is the simplest alcohol in structure, its molecular size is small and can more easily enter the pores of phenolic resin. However, the acetal reaction activity of methanol is low, resulting in the formation of a pore structure that is not stable enough, which is not conducive to the storage of sodium ions. The ultra-low specific surface area carbon material prepared in Comparative Example 2 has closed pores on the surface and an incomplete structure. The molecular size of ethanol is slightly larger than that of methanol, but its acetal reaction activity is higher, and a more stable and more uniform pore structure can be formed. However, ethanol has a high volatility and is easily lost during the curing process, resulting in an incomplete pore structure, which affects the sodium ion storage capacity. The ultra-low specific surface area carbon material prepared in Comparative Example 3 has small pores on the surface, unstable structure, and a large number of collapses. The molecular size of isopropanol is close to that of n-propanol, but its stereo effect makes its acetal reaction more active and easily forms a smaller pore structure. However, these small pore structures are not stable enough, which is not conducive to the storage of sodium ions.
[0042] Effect Example 2: Specific surface area and nitrogen adsorption test
[0043] The specific surface area test and nitrogen adsorption capacity test were carried out for the ultra-low specific surface area carbon materials prepared in Examples 1-5 and Comparative Examples 1-3. The test results are shown in Tables 4 and Figure 2 .
[0044] Table 4 Specific surface area and nitrogen adsorption test results
[0045] Example Group <![CDATA[Specific surface area (m 2 / g)]]> Nitrogen adsorption near P / P0=0 Example 1 10.56 Close to 0 Example 2 10.98 Close to 0 Example 3 10.91 Close to 0 Example 4 9.66 Close to 0 Example 7 9.75 Close to 0 Comparative Example 1 12.52 Close to 0 Comparative Example 2 17.58 Close to 0 Comparative Example 3 14.66 Close to 1
[0046] As shown in Table 4, the specific surface area test shows that the specific surface areas of the ultra-low specific surface area carbon materials prepared in Examples 1-5 are all lower than 12 m 2 / g, while the specific surface areas of the ultra-low specific surface area carbon materials prepared in Comparative Examples 1-3 are all greater than 12 m 2 / g. The results show that the carbon material prepared by the method for preparing the ultra-low specific surface area carbon material of the present application has an extremely low specific surface area, while the carbon materials corresponding to methanol, ethanol and isopropanol are difficult to meet the ultra-low specific surface area requirements.
[0047] like Figure 2 The figure shows the nitrogen adsorption test result of the ultra-low specific surface area carbon material corresponding to Example 3. There is almost no nitrogen adsorption near P / P0=0 in the figure, indicating that the micropores of the ultra-low specific surface area carbon material corresponding to Example 3 are closed-cell structures, and nitrogen cannot enter.
[0048] Comparative Example 3: Charge and Discharge Test
[0049] The ultra-low specific surface area carbon materials prepared in Example 3 and Comparative Examples 1-3, metal lithium sheet counter electrode and 1M LiPF6 electrolyte were assembled into a battery for charge and discharge test, and the charge and discharge curves were plotted. The results are shown in Table 5 and Figure 3 shown.
[0050] Table 5 Charge and discharge test results
[0051] Example Group First charge specific capacity (mAh / g) First discharge specific capacity (mAh / g) First charge and discharge efficiency (%) Example 3 412.0 384.8 93.4 Comparative Example 1 407.2 347.2 85.3 Comparative Example 2 422.5 356.1 84.3 Comparative Example 3 429.7 332.1 77.3
[0052] As shown in Table 5, the batteries using the ultra-low specific surface area carbon materials prepared in Example 3 and Comparative Examples 1-3 as negative electrodes have similar first charge specific capacities. However, in terms of first discharge specific capacity, the battery corresponding to Example 3 is significantly higher than the batteries corresponding to Comparative Examples 1-3, and the first charge and discharge efficiency of the battery corresponding to Example 3 is significantly higher than the batteries corresponding to Comparative Examples 1-3.
[0053] like Figure 3 As shown, it is the charge and discharge curve of the battery corresponding to Example 3, showing that the first charge specific capacity is 412.0 mAh / g, the first discharge specific capacity is 384.8 mAh / g, and the first charge and discharge efficiency is 93.4%.
[0054] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing an ultra-low specific surface area carbon material, characterized in that: The following steps are included by weight: Preparation of a closed-cell material: providing 10 to 50 parts of a thermoplastic phenolic resin and 10 parts of a closed-cell agent, mixing the thermoplastic phenolic resin and the closed-cell agent to obtain a mixed system, transferring the mixed system to 150 to 250° C. for hydrothermal reaction for 1 to 12 hours, and then transferring the mixed system to 80 to 150° C. for drying for 2 to 12 hours to obtain a closed-cell material; Preparation of ultra-low specific surface area carbon material: placing the closed-cell material in an inert atmosphere at 1200-1700° C. for carbonization for 1-4 hours to obtain an ultra-low specific surface area carbon material; The cell-blocking agent is n-propanol.
2. The method for preparing the ultra-low specific surface area carbon material according to claim 1, characterized in that: In the step of preparing the closed-cell material, the amount of the thermoplastic phenolic resin is 15 to 25 parts, the mixed system is transferred to 160 to 200° C. for hydrothermal reaction for 2 to 8 hours, and then the mixed system is transferred to 100 to 130° C. for drying for 4 to 8 hours.
3. The method for preparing the ultra-low specific surface area carbon material according to claim 2, characterized in that: In the step of preparing the closed-cell material, the amount of the thermoplastic phenolic resin used is 20 parts, the mixed system is transferred to 180° C. for hydrothermal reaction for 4 hours, and then the mixed system is transferred to 120° C. for vacuum drying for 6 hours.
4. The method for preparing the ultra-low specific surface area carbon material according to claim 1, characterized in that: In the step of preparing the ultra-low specific surface area carbon material, the closed-cell material is placed in a tubular furnace and the tubular furnace is filled with an inert gas, wherein the inert gas is nitrogen or argon. The tubular furnace is then heated to 1200-1700° C. and maintained for 1-4 hours to obtain the ultra-low specific surface area carbon material.
5. The method for preparing the ultra-low specific surface area carbon material according to claim 4, characterized in that: In the step of preparing the ultra-low specific surface area carbon material, the tubular furnace is heated to 1500° C. and maintained for 2 hours, the heating rate is 2° C. / min, and the ultra-low specific surface area carbon material is obtained after natural cooling.
6. An ultra-low specific surface area carbon material, characterized in that: The carbon material is prepared by the method for preparing the ultra-low specific surface area carbon material according to any one of claims 1 to 5.
7. The ultra-low specific surface area carbon material according to claim 6, characterized in that: The specific surface area of the ultra-low specific surface area carbon material is not more than 12 m 2 / g.
8. A battery, characterized in that: Including the ultra-low specific surface area carbon material as described in claim 6 or 7.
Citation Information
Patent Citations
Sodium-ion battery hard carbon negative electrode material with ultralow specific surface area and preparation method of sodium-ion battery hard carbon negative electrode material
CN115207350A
Preparation method of negative electrode material for sodium ion battery
CN116177528A