Preparation method of mesoporous carbon black for fuel cell
Through the soft template pore making and segmented heat treatment method of mesoporous carbon black, the problem of low performance of platinum carbon catalyst in fuel cells is solved, and the uniform dispersion of platinum particles and the improvement of catalyst performance is achieved, which is suitable for industrial production and reduces costs.
Patent Information
- Application Number
- CN202411050669.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The mass transfer efficiency of platinum carbon catalysts in existing fuel cells is low, the platinum particles are uneven or too large, resulting in low catalyst performance and few research on the development of new carbon black support, affecting the performance of platinum carbon catalysts.
A mesoporous carbon black preparation method is adopted to regulate the pore structure and particle size of the carbon black carrier through soft template pore formation and segmented heat treatment, improve the uniform dispersion and graphitization of platinum particles, and combine low-temperature and high-temperature treatment to remove impurities , enhance the performance of the catalyst.
It effectively improves the uniform dispersion of platinum particles and catalyst performance, reduces production costs, realizes the feasibility of industrial production, and improves the mass transfer capacity of platinum carbon catalysts.
Smart Images

Figure CN118978143A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of carbon black carrier for fuel cells, and in particular to a method for preparing mesoporous carbon black for fuel cells. Background Art
[0002] As the world's requirements for carbon emissions become increasingly stringent and the country's urgent need for green energy, hydrogen fuel cells are favored by people for their green environmental protection and high energy conversion efficiency, and are expected to become an important pillar of green energy in the future. The platinum-carbon catalyst used in the cathode of the fuel cell is the core component of the battery. However, the platinum-carbon catalyst is affected by the carbon black carrier during the application process, which will lead to low mass transfer efficiency, uneven or too large platinum particles, etc., resulting in low catalyst performance. The mesoporous carbon black carrier has a suitable pore structure that can ensure timely discharge of water at high electric density to improve mass transfer efficiency. At the same time, the appropriate pore size can ensure that the platinum particles in the catalyst are evenly loaded and the particle size is controllable, thereby improving the catalyst performance.
[0003] At present, a large number of studies are mainly focused on the surface modification of carbon black carriers. By changing the surface properties of carbon black carriers and changing the loading process of platinum particles during catalyst synthesis, the catalyst is optimized. There are few studies on the development of new carbon black carriers. Carbon black carriers are an important factor affecting the performance of platinum-carbon catalysts. Carbon black carriers with different structures have a great influence on the performance of platinum-carbon catalysts. Therefore, a new method for preparing carbon black carriers is needed to prepare new carbon black carriers. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention aims to provide a method for preparing mesoporous carbon black for fuel cells.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing mesoporous carbon black for fuel cells comprises the following steps:
[0007] S1, adding a polymer precursor and formaldehyde solution into deionized water;
[0008] S2, slowly dropwise adding sodium hydroxide solution, reacting at 100°C to obtain solution A;
[0009] S3, adding an excess amount of surfactant to deionized water, then adding p-xylene, stirring at room temperature to prepare solution B;
[0010] S4, adding solution B to solution A, stirring and reacting at 80°C;
[0011] S5, adding hydrochloric acid solution dropwise and stirring to obtain a gel;
[0012] S6, placing the gel in a forced air drying oven and drying at 120° C. to obtain a black precursor C;
[0013] S7, placing the black precursor C in a ball mill for ball milling, and then placing it in a tube furnace for heat treatment at 350° C. under an inert atmosphere;
[0014] S8. Continue to raise the temperature to 900° C. for carbonization to obtain mesoporous carbon black for fuel cells.
[0015] It should be noted that the purpose of first mixing the polymerization precursor and formaldehyde solution and adding sodium hydroxide is to adjust the pH of the reaction system to form a prepolymer and accelerate the subsequent polymerization reaction. The main purpose of the excess surfactant is to form stable micelles at a certain concentration, so that the prepared carbon black carrier will obtain a relatively uniform pore structure and pore size distribution. The purpose of adding hydrochloric acid solution is mainly to condense the prepolymer to form a resin and provide an environment for the polymerization reaction to occur. The purpose of the segmented heat treatment is to first remove the residual reactants and impurities such as water in the resin to avoid subsequent carbonization leading to clogging of the carbon black carrier pores and structural deformation.
[0016] Furthermore, in step S1, the polymer precursor includes one or more of pyrrole, melamine, dopamine, polydopamine, and aniline.
[0017] Furthermore, the concentration of the formaldehyde solution is 10%-37%, the concentration of the sodium hydroxide solution is 0.1mol / L-3mol / L; the concentration of the hydrochloric acid solution is 0.1mol / L-1mol / L; the mass ratio of the polymerization precursor, formaldehyde solution, sodium hydroxide solution, p-xylene and hydrochloric acid solution is 5:1:1-4:0.3:3.
[0018] Furthermore, in step S3, the surfactant includes one or more of polyethyleneimine, polyoxyethylene polyoxypropylene ether, polyethylene oxide polypropylene oxide, hexadecyltrimethylammonium bromide, sodium dodecylbenzene sulfonate, and polyetherimide.
[0019] Furthermore, in step S7, the ball milling speed is 400 rpm and the ball milling time is 4 h.
[0020] The beneficial effects of the present invention are:
[0021] 1) The method of the present invention adopts a soft template pore-forming method, which can regulate the pores of the carbon black carrier by controlling the amount of surfactant added as a soft template, which can effectively improve the uniform dispersion of platinum particles and has a good effect on improving the catalyst performance.
[0022] 2) The present invention selects a segmented heat treatment method in the carbonization stage, removes impurities in the carrier by combining low temperature and high temperature, and improves the graphitization degree of the carbon black carrier. At the same time, the carbon black carrier particles partially shrink in the high temperature zone, and the reduction of the carrier particle size can effectively improve the mass transfer capacity of the carrier.
[0023] 3) The method of the present invention has relatively mild conditions, and the prepared carbon black carrier particles have good consistency, which can be industrialized and at a low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The voltammetric cycle curve of the platinum-carbon catalyst prepared by using the carbon black carrier obtained in Example 2 of the present invention;
[0025] Figure 2 This is a diagram of the oxygen reduction polarization curve of the platinum-carbon catalyst prepared using the carbon black carrier obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0027] Example 1
[0028] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0029] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0030] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0031] S3. Add 1 g of polyethyleneimine to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0032] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0033] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0034] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0035] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0036] S8. Continue to raise the temperature to 900° C. for carbonization to obtain mesoporous carbon black for fuel cells.
[0037] Example 2
[0038] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0039] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0040] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0041] S3. Add 2 g of polyethyleneimine to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0042] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0043] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0044] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0045] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0046] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0047] Example 3
[0048] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0049] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0050] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0051] S3. Add 4 g of polyethyleneimine to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0052] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0053] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0054] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0055] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0056] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0057] Example 4
[0058] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0059] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0060] S2. Slowly drop 2 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0061] S3. Add 2 g of polyethyleneimine to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0062] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0063] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0064] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0065] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0066] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0067] Example 5
[0068] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0069] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0070] S2. Slowly drop 4 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0071] S3. Add 2 g of polyethyleneimine to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0072] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0073] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0074] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0075] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0076] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0077] Example 6
[0078] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0079] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0080] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0081] S3. Add 2 g of polyoxyethylene polyoxypropylene ether to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0082] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0083] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0084] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0085] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0086] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0087] Example 7
[0088] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0089] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0090] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0091] S3. Add 2 g of sodium dodecylbenzene sulfonate to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0092] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0093] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0094] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0095] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0096] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0097] Example 8
[0098] This embodiment provides a method for preparing mesoporous carbon black for fuel cells, comprising the following steps:
[0099] S1. Add 5 g of pyrrole and 1 g of 15% formaldehyde solution into 800 g of deionized water and stir evenly.
[0100] S2. Slowly drop 1 g of 0.1 mol / L sodium hydroxide solution, heat in a water bath at 100° C. and stir for 1.5 h to obtain solution A.
[0101] S3. Add 2 g of polyethylene oxide and polypropylene oxide to 0.5 g of deionized water, then add 0.3 g of p-xylene, and stir at room temperature for 3 h to obtain solution B.
[0102] S4. Add solution B into solution A and stir the mixture at 80°C for 2 h.
[0103] S5. Add 3 g of 0.15 mol / L hydrochloric acid solution dropwise and stir for 3 h to obtain a gel.
[0104] S6. Place the gel in a forced air drying oven and dry at 120° C. for 24 h to obtain a black precursor C.
[0105] S7. The black precursor C is placed in a ball mill for ball milling, and then placed in a tubular furnace for heat treatment at 350° C. for 2 h under an inert atmosphere.
[0106] S8. Continue to raise the temperature to 900° C. for carbonization to obtain a carbon black carrier sample containing mesopores.
[0107] The mesoporous carbon black carrier prepared in the above embodiment is prepared into a platinum-carbon catalyst with a platinum loading of 50%, and the platinum-carbon catalyst is subjected to an RDE performance test to determine its performance, thereby evaluating the effect of the carbon black carrier on the platinum-carbon catalyst. The preparation process of the platinum-carbon catalyst is as follows:
[0108] 3.4g of CTAB and 3.5g of carbon black carrier were dispersed in 150g of deionized water and stirred for 1h to obtain suspension C, and then 10g of chloroplatinic acid was dissolved in 300g of deionized water to obtain solution D. Solution D was poured into suspension C, stirred and mixed at 80°C for 3h, and then the reaction solution was cooled to room temperature. 22g of sodium borohydride solution with a concentration of 20% was prepared. 22g of sodium borohydride solution was slowly added dropwise to the reaction solution, and the reaction was stirred in an oil bath at 60°C for 2h. After the reaction was completed and cooled to room temperature, the product solution was separated by suction filtration with deionized water. The filter cake obtained by suction filtration was placed in a 500ml beaker, about 500ml of deionized water was added, stirred and ultrasonically dispersed for 30min, and then separated by suction filtration again. Repeat the above operation until the conductivity of the filtrate is less than 50S / cm. Then take out the sample and dry it in a blast drying oven at 120°C for 12h. The dried sample was ground using a mortar to obtain a catalyst powder sample with a platinum loading of 50%.
[0109] The specific electrochemical performance of the platinum-carbon catalyst prepared using the carbon black carrier obtained in Examples 1-8 is shown in Table 1. It can be seen that the electrochemical active area and mass activity of the catalyst prepared in Example 2 are the highest. The average particle size of the platinum particles in the platinum-carbon catalyst can be further calculated based on the XRD pattern, as shown in Table 2.
[0110] Figure 1 and Figure 2 Shown are the voltammetric cycle curve and oxygen reduction polarization curve of the platinum-carbon catalyst prepared using the carbon black carrier obtained in Example 2.
[0111] Table 1
[0112]
[0113]
[0114] Table 2
[0115]
[0116] According to the data in Table 2, it can be found that the particle size of the platinum particles of the platinum-carbon catalyst prepared by the carbon black carrier obtained in Example 2 is 3.7 nm, indicating that different carbon black carrier structures can well control the particle size of the catalyst platinum particles and further affect the catalytic activity, which is also mutually confirmed by the results of the electrochemical test.
[0117] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing mesoporous carbon black for fuel cells, It is characterized in that The following steps are involved: S1, adding a polymer precursor and formaldehyde solution into deionized water; S2, slowly dropwise adding sodium hydroxide solution, reacting at 100°C to obtain solution A; S3, adding an excess amount of surfactant to deionized water, then adding p-xylene, stirring at room temperature to prepare solution B; S4, adding solution B to solution A, stirring and reacting at 80°C; S5, adding hydrochloric acid solution dropwise and stirring to obtain a gel; S6, placing the gel in a forced air drying oven and drying at 120° C. to obtain a black precursor C; S7, placing the black precursor C in a ball mill for ball milling, and then placing it in a tube furnace for heat treatment at 350° C. under an inert atmosphere; S8. Continue to raise the temperature to 900° C. for carbonization to obtain mesoporous carbon black for fuel cells.
2. The preparation method according to claim 1, It is characterized in that In step S1, the polymer precursor includes one or more of pyrrole, melamine, dopamine, polydopamine, and aniline.
3. The preparation method according to claim 1, It is characterized in that The concentration of the formaldehyde solution is 10%-37%, the concentration of the sodium hydroxide solution is 0.1mol / L-3mol / L; the concentration of the hydrochloric acid solution is 0.1mol / L-1mol / L; the mass ratio of the polymerization precursor, the formaldehyde solution, the sodium hydroxide solution, p-xylene and the hydrochloric acid solution is 5:1:1-4:0.3:
3.
4. The preparation method according to claim 1, It is characterized in that In step S3, the surfactant includes one or more of polyethyleneimine, polyoxyethylene polyoxypropylene ether, polyethylene oxide polypropylene oxide, hexadecyltrimethylammonium bromide, sodium dodecylbenzene sulfonate, and polyetherimide.
5. The preparation method according to claim 1, It is characterized in that In step S7, the ball milling speed is 400 rpm and the ball milling time is 4 h.
Citation Information
Patent Citations
Ultralow-platinum fuel cell catalyst and preparation method thereof
CN115133051A
Electrode catalyst for fuel cell, process for producing the same and fuel cell utilizing the catalyst
WO2006003831A1