Defective ZnMn2O4 material, preparation method thereof and application of defective ZnMn2O4 material as positive electrode of aqueous zinc ion battery
By adjusting the ratio of manganese zinc compounds in an organic solvent and heating in a room temperature water bath, the cation defective ZnMn2O4 positive electrode material is solved, and the problems of insufficient performance of the positive electrode material and complex preparation process in the prior art are achieved, and a high-efficiency and low-cost water-based zinc ion battery is achieved. The preparation of the positive electrode material improves the circulation performance and energy density of the battery.
Patent Information
- Application Number
- CN202410877940.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-19
AI Technical Summary
The existing positive electrode materials of zinc ion batteries in water system have problems such as low rate performance and capacity, slow reaction kinetics and short cycle life. The commonly used preparation methods are costly, long cycles and cumbersome, which limit the development and application of materials.
By adjusting the ratio of manganese source compound and zinc source compound in an organic solvent, heating at room temperature, combined with centrifugation and vacuum drying, a cationic defective ZnMn2O4 cathode material is prepared, simplifying the preparation process and reducing costs.
It achieves high specific capacity (266.2mAh/g) and excellent cycling performance, improves the rate performance and energy density of the battery, and has simple process, low equipment requirements and small energy consumption.
Smart Images

Figure CN118978184A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and specifically relates to a defective ZnMn2O4 material and a preparation method thereof, and an application thereof as a positive electrode of an aqueous zinc ion battery. Background Art
[0002] Aqueous zinc-ion batteries (AZIBs) are considered to be one of the most competitive candidate energy storage systems due to their high safety, high theoretical specific capacity (820mAh / g), low redox potential (-0.76Vvs.SHE), high natural abundance of Zn, and environmental friendliness. Among them, the positive electrode material is the main factor affecting the performance of AZIBs, and people have made great efforts to explore and design efficient positive electrode materials for AZIBs. The ideal positive electrode material must have a suitable open framework and a solid structure that can reversibly accommodate Zn during the charge and discharge process. 2+ . Currently, the widely studied cathode materials can be roughly divided into manganese-based oxides, vanadium-based oxides, Prussian blue analogs and organic compounds. However, these cathode materials have disadvantages such as low rate performance and capacity, slow reaction kinetics and short cycle life, which limit the development of AZIBs. Therefore, the development of new and efficient cathode materials is one of the key points to realize the commercialization of AZIBs.
[0003] Spinel-structured zinc manganese oxide (ZnMn2O4) is a promising cathode material in AZIBs due to its considerable capacity and suitable redox potential. 2+ The huge electrostatic interaction force during the embedding / extraction process will lead to slow electrochemical kinetics of the battery. In addition, ZnMn2O4 has problems such as manganese dissolution common in manganese-based materials and poor conductivity inherent in transition metal oxides, which further lead to capacity decay of ZnMn2O4 cathode materials during long-term cycling. Studies have found that the introduction of cation defects can induce electron rearrangement, improve conductivity and ion diffusion, and thus improve the electrochemical performance of the battery. This is of great significance for the development of high-safety, low-cost and environmentally friendly AZIBs. At present, defects are mainly introduced into ZnMn2O4 by hydrothermal method, calcination or electrochemical deposition, but these methods are costly, have long experimental cycles and cumbersome preparation processes, which limit the development and application of materials. Therefore, it is urgent to develop a ZnMn2O4 cathode material with simple preparation process, high yield, low cost and excellent Zn storage performance, which is of great significance for the realization of high-performance AZIBs. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0006] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a defective ZnMn2O4 material and a preparation method thereof and an application thereof as a positive electrode of an aqueous zinc ion battery. The present invention adjusts the ratio of a manganese source compound and a zinc source compound, directly performs water bath heating in an organic solvent, and has a simple preparation process and low cost, and is a feasible method for preparing a defective ZnMn2O4 positive electrode material.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:
[0008] The manganese source compound is placed in an organic solvent and stirred to dissolve;
[0009] The zinc source compound is added to the solution and stirred until completely dissolved to obtain a mixed solution I;
[0010] The mixed solution I is stirred at room temperature in a water bath at 40 to 90° C. for 3 to 10 hours to obtain a mixture;
[0011] The precipitate of the mixture is collected by centrifugation, washed by centrifugation with deionized water and ethanol respectively, and vacuum dried to obtain the cation-deficient ZnMn2O4 positive electrode material.
[0012] As a preferred scheme for the preparation method of the defective ZnMn2O4 material described in the present invention, the manganese source compound includes one or more of KMnO4, Mn(NO3)2·4H2O, MnCl2, MnSO4·4H2O or (CH3COO)2Mn·4H2O, more preferably KMnO4 and MnSO4·4H2O.
[0013] As a preferred embodiment of the method for preparing the defective ZnMn2O4 material described in the present invention, the organic solvent comprises one of methanol, ethanol, ethylene glycol, propylene glycol, n-butanol, and benzyl alcohol, and more preferably comprises one of methanol, ethanol or propylene glycol.
[0014] As a preferred scheme of the preparation method of the defective ZnMn2O4 material described in the present invention, the volume of organic solvent required for every 1 mmol of the zinc source compound is 5 to 45 mL, and more preferably, the volume of organic solvent required for every 1 mmol of the zinc source compound is 12.5 to 37.5 mL.
[0015] As a preferred scheme for the preparation method of the defective ZnMn2O4 material described in the present invention, the zinc source compound includes one or more of ZnSO4·7H2O, (CH3COO)2Zn·2H2O, Zn(NO3)2·6H2O or ZnCl2, and more preferably includes one of ZnSO4·7H2O or Zn(NO3)2·6H2O.
[0016] As a preferred embodiment of the method for preparing the defective ZnMn2O4 material of the present invention, the molar ratio of the manganese source compound to the zinc source compound is 1.5 to 6:1, more preferably 2.5 to 3:1.
[0017] As a preferred solution of the method for preparing the defective ZnMn2O4 material described in the present invention, the temperature of the water bath is 40-90°C, more preferably 55-75°C.
[0018] As a preferred solution of the method for preparing the defective ZnMn2O4 material described in the present invention, the stirring time in the water bath is 3 to 10 hours, more preferably 4 to 6 hours.
[0019] As a preferred solution of the method for preparing the defective ZnMn2O4 material described in the present invention, the vacuum drying atmosphere is one of oxygen, nitrogen and argon, and more preferably includes one of oxygen or nitrogen.
[0020] As a preferred solution of the method for preparing the defective ZnMn2O4 material described in the present invention, the vacuum drying temperature is 60-90°C, more preferably 70-80°C.
[0021] As a preferred solution of the method for preparing the defective ZnMn2O4 material described in the present invention, the vacuum drying time is 8 to 16 hours, more preferably 10 to 12 hours.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a defective ZnMn2O4 material for use as a positive electrode for an aqueous zinc ion battery.
[0023] Beneficial effects of the present invention:
[0024] (1) The preparation method of the present invention first mixes the samples at room temperature, and then obtains the ZnMn2O4 positive electrode material with cation defects by water bath heating, centrifugation, and vacuum drying. Compared with the commonly used high temperature and high pressure hydrothermal (solvothermal) method combined with a subsequent heat treatment process, the preparation process is simple, the equipment requirements are low, the reaction conditions are mild, and the energy consumption is low.
[0025] (2) The preparation method of the present invention uses an organic solvent as a reaction solvent, and does not require the addition of additional surfactants and reducing agents, and does not require doping or compounding with other materials to obtain a defective ZnMn2O4 positive electrode material.
[0026] (3) After 100 cycles of rate charge and discharge combined with constant current charge and discharge test, the ZnMn2O4 cathode material with cation defects prepared by the method of the present invention has a specific capacity of up to 266.2 mAh / g at a current density of 0.8 A / g. This is because by introducing defects in the lattice, the transport kinetics of ions in the cathode material can be accelerated, thereby showing excellent specific capacity, cycle performance and rate performance, and the energy density is also enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0028] Figure 1 It is the X-ray diffraction pattern of the defective ZnMn2O4 positive electrode material prepared in Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1.
[0029] Figure 2 This is a scanning electron microscope image of the defective ZnMn2O4 positive electrode material prepared in Example 1.
[0030] Figure 3 It is the X-ray photoelectron spectrum of the cation-defective ZnMn2O4 prepared in Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1.
[0031] Figure 4 It is the electron paramagnetic resonance image of the cation-deficient ZnMn2O4 prepared in Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1.
[0032] Figure 5 This is the cycle performance diagram of the cation-deficient ZnMn2O4 prepared in Example 1.
[0033] Figure 6It is a cycle performance diagram of the defective ZnMn2O4 positive electrode materials prepared in Example 13, Example 15 and Example 17 and the defect-free ZnMn2O4 prepared in Comparative Example 1. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0036] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0037] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art.
[0038] Example 1
[0039] Place 6 mmol of KMnO4 in 60 mL of ethanol, stir at room temperature until dissolved, then add 2 mmol of ZnSO4·7H2O and continue stirring until dissolved;
[0040] The obtained solution was stirred in a 60°C water bath for 6 h and then centrifuged to collect the precipitate;
[0041] The collected precipitate was placed in a vacuum drying oven at 70° C. under an oxygen atmosphere and dried for 12 hours to obtain the target product cation-deficient ZnMn2O4, wherein the molar ratio of the manganese source compound to the zinc source compound was 3:1.
[0042] Depend on Figure 1 It can be seen from the X-ray diffraction pattern that the ZnMn2O4 with cation defects prepared in this embodiment has good crystallinity, the diffraction peak position matches the JCPDS No.24-1133 (ZnMn2O4) standard spectrum, and no impurity peaks appear, indicating that a pure phase ZnMn2O4 positive electrode material is successfully prepared.
[0043] Depend on Figure 2 Scanning electron microscopy shows that the ZnMn2O4 with cation defects prepared in this example has an irregular three-dimensional structure.
[0044] Depend on Figure 3 X-ray photoelectron spectroscopy and Figure 4 It can be seen from the electron paramagnetic resonance image that the cation-deficient ZnMn2O4 prepared in this example has abundant oxygen vacancies.
[0045] Depend on Figure 5 It can be seen from the cycle performance diagram that when the ZnMn2O4 material with cation defects prepared in this embodiment is used as the positive electrode of AZIBs, at a current density of 0.8A / g, after 100 cycles, the specific capacity still reaches 266.2mAh / g, and the charge and discharge efficiency is close to 100%, showing good cycle stability and excellent rate performance.
[0046] Comparative Example 1
[0047] This comparative example is to synthesize ZnMn2O4 without defects, and the specific steps are as follows:
[0048] Place 6 mmol of KMnO4 in 60 mL of ethanol, stir at room temperature until dissolved, then add 3 mmol of ZnSO4·7H2O and continue stirring until dissolved;
[0049] The obtained solution was stirred in a 60°C water bath for 6 h and then centrifuged to collect the precipitate;
[0050] The collected precipitate was placed in a vacuum drying oven at 70°C under an oxygen atmosphere and dried for 12 hours to obtain the target product, defect-free ZnMn2O4.
[0051] Example 2
[0052] The difference between this embodiment and embodiment 1 is that the organic solvent is adjusted to methanol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0053] Example 3
[0054] The difference between this embodiment and embodiment 1 is that the organic solvent is adjusted to ethylene glycol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0055] Example 4
[0056] The difference between this embodiment and embodiment 1 is that the organic solvent is adjusted to propylene glycol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0057] Example 5
[0058] The difference between this embodiment and embodiment 1 is that the organic solvent is adjusted to n-butanol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0059] Example 6
[0060] The difference between this embodiment and embodiment 1 is that the organic solvent is adjusted to benzyl alcohol, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0061] The performance comparison of the cation-defective ZnMn2O4 prepared using different organic solvents in Examples 1 to 6 and the defect-free ZnMn2O4 prepared in Comparative Example 1 is shown in Table 1.
[0062] Table 1 Effects of different organic solvents on the properties of the prepared materials
[0063]
[0064] It can be seen from Table 1 that adjusting the type of solvent has a significant effect on the positive electrode material. This may be because the number and position of the methyl groups therein have a certain influence on the solute. According to the results in Table 1, better technical effects can be obtained when ethanol is used as the organic solvent.
[0065] Example 7
[0066] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 15 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0067] Example 8
[0068] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 30 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0069] Example 9
[0070] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 45 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0071] Example 10
[0072] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 65 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0073] Embodiment 11
[0074] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 80 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0075] Example 12
[0076] The difference between this embodiment and embodiment 1 is that the volume of the organic solvent ethanol is adjusted to 90 mL, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0077] Comparative Example 2
[0078] The difference between this comparative example and Example 1 is that the volume of ethanol is adjusted to 5 mL and 95 mL, and the rest of the preparation process is the same as Example 1. The purity of the prepared ZnMn2O4 material is low and subsequent performance testing cannot be carried out.
[0079] Table 2 shows a comparison of the properties of the cation-defective ZnMn2O4 prepared with different volumes of organic solvents in Examples 7 to 12 and Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1.
[0080] Table 2 Effect of different solvent volumes on the properties of the prepared materials
[0081]
[0082] It can be seen from Table 2 that different solvent volumes have a significant effect on the positive electrode material. This may be because different solvent volumes have different solubility for zinc / manganese source compounds. According to the results in Table 2, better technical effects can be obtained when the volume of the organic solvent in the present invention is 60 mL.
[0083] Embodiment 13
[0084] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 3 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 1.5:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0085] Embodiment 14
[0086] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 4.5 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 2.25:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0087] Embodiment 15
[0088] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 7.5 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 3.75:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0089] Example 16
[0090] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 8 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 4:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0091] Embodiment 17
[0092] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 10.5 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 5.25:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0093] Embodiment 18
[0094] The difference between this embodiment and embodiment 1 is that the addition amount of KMnO4 is adjusted to 12 mmol, that is, the molar ratio of the manganese source compound to the zinc source compound is 6:1, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0095] Comparative Example 3
[0096] The difference between this comparative example and Example 1 is that the addition amount of KMnO4 is adjusted to 2 mmol and 12.5 mmol, that is, the molar ratios of the manganese source compound and the zinc source compound are 1:1 and 6.25:1 respectively, and the rest of the preparation process is the same as Example 1. The purity of the prepared ZnMn2O4 material is low and subsequent performance testing cannot be carried out.
[0097] The performance comparison of the cation-deficient ZnMn2O4 prepared using different manganese-zinc molar ratios in Examples 13 to 18 and Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1 is shown in Table 3.
[0098] Table 3 Effect of different molar ratios of manganese and zinc on the properties of the obtained materials
[0099]
[0100] It can be seen from Table 3 that the molar ratio of the manganese source compound to the zinc source compound has a significant effect on the positive electrode material. This is because different molar ratios form different types of defects and have different effects on the performance of the positive electrode material. According to the results in Table 3, when the molar ratio of the manganese source compound to the zinc source compound in the present invention is 3:1, better technical effects can be obtained.
[0101] Embodiment 19
[0102] The difference between this embodiment and embodiment 1 is that the added zinc source compound is adjusted to (CH3COO)2Zn·2H2O, and the rest of the preparation process is the same as that of embodiment 1, to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0103] Embodiment 20
[0104] The difference between this embodiment and embodiment 1 is that the added zinc source compound is adjusted to Zn(NO3)2·6H2O, and the rest of the preparation process is the same as that of embodiment 1, to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0105] Embodiment 21
[0106] The difference between this embodiment and embodiment 1 is that the added zinc source compound is adjusted to ZnCl2, and the rest of the preparation process is the same as that of embodiment 1 to obtain the cation-deficient ZnMn2O4 of this embodiment.
[0107] The performance comparison of the cation-deficient ZnMn2O4 prepared using different zinc source compounds in Examples 19 to 21 and Example 1 and the defect-free ZnMn2O4 prepared in Comparative Example 1 is shown in Table 4.
[0108] Table 4 Effect of different zinc source compounds on the properties of the prepared materials
[0109]
[0110] It can be seen from Table 4 that different types of zinc source compounds also have a certain degree of influence on the performance of the battery. According to the results in Table 4, better technical effects can be obtained when the zinc source compound used is ZnSO4·7H2O.
[0111] Embodiment 22
[0112] This embodiment is the assembly and testing of a zinc ion battery.
[0113] Electrochemical tests were performed using button cells. To prepare the working electrode, the active material, acetylene black, and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 7:2:1 to prepare a uniform slurry. The resulting slurry was then coated on a titanium foil and vacuum dried at 80°C for 8h. The battery used zinc metal as the negative electrode and then assembled the battery.
[0114] The defective ZnMn2O4 prepared in Example 1, Example 13, and Example 17 and the defect-free ZnMn2O4 prepared in Comparative Example 1 were used as active materials to test the electrochemical properties. Figure 6 The figure is the electrochemical performance diagram of the discharge capacity changing with the number of cycles. The current density used in the test is 0.8A / g. It can be clearly seen that with the increase of the molar ratio of manganese zinc compound, the discharge capacity increases from 201.4mAh / g to 266.2mAh / g. Figure 6 It can be clearly seen that the prepared defective ZnMn2O4 has a discharge capacity of more than 30 mAh / g higher than that of the defect-free type after cycling. This is attributed to the fact that the prepared defective ZnMn2O4 can accelerate the reaction kinetics of ion transport and alleviate the capacity decay caused by volume expansion caused by the de-insertion of zinc.
[0115] In summary, the present invention mixes the samples at room temperature, and then obtains ZnMn2O4 positive electrode materials with cation defects by water bath heating, centrifugation, and vacuum drying. The present invention accelerates the ion transport kinetics in the positive electrode material by introducing defects in the lattice, thereby showing excellent specific capacity, cycle performance and rate performance, and also enhancing the energy density.
[0116] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A defective ZnMn 2 O 4 Methods of preparing materials, Features: include, Add the manganese source compound to the organic solvent and stir until dissolved; Adding a zinc source compound and dissolving it in the above solution to obtain a mixed solution I; The molar ratio of the manganese source compound to the zinc source compound is 1.5 to 6:1, and the volume of the organic solvent required for each 1 mmol of the zinc source compound is 5 to 45 mL; The mixed solution I was stirred in a water bath, the precipitate was collected by centrifugation, and the gas was passed through for vacuum drying to obtain ZnMn with cation defects. 2 O 4 Material.
2. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The manganese source compound includes KMnO 4 、Mn(NO 3 ) 2 ·4H 2 O、MnCl 2 、MnSO 4 ·4H 2 O or (CH 3 COO 2 Mn·4H 2 One or more of O.
3. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The organic solvent includes one or more of methanol, ethanol, ethylene glycol, glycerol, n-butanol or benzyl alcohol.
4. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The volume of the organic solvent required for each 1 mmol of the zinc source compound is 12.5 to 37.5 mL.
5. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The zinc source compound includes ZnSO 4 7H 2 O、(CH 3 COO 2 Zn·2H 2 O、Zn(NO 3 ) 2 6H 2 O or ZnCl 2 One or more of .
6. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The molar ratio of the manganese source compound to the zinc source compound is 2.5 to 3:
1.
7. The defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The temperature of the water bath is 40-90° C., and the stirring time in the water bath is 3-10 hours.
8. Defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The introduced gas includes one or more of oxygen, nitrogen or argon.
9. The defective ZnMn as claimed in claim 1 2 O 4 Methods of preparing materials, Features: The vacuum drying is carried out at a temperature of 60 to 90° C. and for a time of 8 to 16 hours.
10. The defective ZnMn according to any one of claims 1 to 9 2 O 4 Application of the material as positive electrode for aqueous zinc-ion batteries.