Lithium-rich manganese-based precursor material and preparation method thereof
By preparing lithium-rich manganese-based precursor material with the chemical formula of NixMn(1-x)(OH)2 of hydroxide, the problems of poor spherical shape and low tap density in the prior art are solved, and uniform particle size and high tap density are achieved. The material preparation simplifies the process flow, is suitable for industrial production and improves electrochemical performance.
Patent Information
- Application Number
- CN202410651255.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-19
AI Technical Summary
The existing precursor preparation technology for lithium-rich manganese-based materials has problems such as poor spherical shape, low tap density, and coarse primary particles, which affect the processing performance of the material and the volume energy density of the battery, and organic complexing agents are often required to increase production. Cost and water treatment burden.
By preparing lithium-rich manganese-based precursor material with the chemical formula of NixMn(1-x)(OH)2, the soluble salt dissolution of nickel and manganese, the preparation of sodium hydroxide and ammonia water is controlled to control the reaction temperature, pH value and Ammonia concentration, stirring and filtering using a synthetic device, and finally drying and sieving to obtain a precursor material with uniform particle size and high tap density.
It realizes the preparation of lithium-rich manganese-based precursor materials with high uniform particle size and high tap density, simplifies the process flow, avoids the use of surfactants and crystal growth guides, is suitable for industrial production, and improves the electrochemical performance and production of the materials. efficiency.
Smart Images

Figure CN118978190A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium-rich manganese-based precursor materials, and in particular to a lithium-rich manganese-based precursor material and a preparation method thereof. Background Art
[0002] As a new type of green energy, lithium-ion batteries have the advantages of high specific energy and long cycle life. They are widely used by the battery industry as a new type of green battery. For example, lithium-ion batteries are widely used in the digital field, electric vehicle field, energy storage field, etc. As an important component of lithium-ion batteries, positive electrode materials have a crucial impact on the electrochemical properties of lithium-ion batteries. Nickel-cobalt-manganese ternary positive electrode material is one of the main positive electrode materials for lithium-ion batteries at present, with the characteristics of high specific capacity and good cycle stability.
[0003] Compared with nickel-cobalt-manganese ternary lithium batteries, lithium-rich manganese-based lithium batteries have attracted widespread attention in recent years due to their high reversible specific capacity, excellent cycle performance, relatively low cost, and new electrochemical charge and discharge mechanisms. They are considered to be one of the key positive electrode materials for the next generation of high-energy lithium-ion batteries.
[0004] However, the preparation technology of lithium-rich manganese-based materials and their precursors is still immature, which restricts their large-scale and commercial application. When using a hydroxide precursor preparation process similar to nickel-cobalt-manganese ternary materials, due to the high manganese content in lithium-rich manganese-based materials, Mn 2+ Ions nucleate too quickly during the precipitation process, which can easily generate large primary flake MnOOH. Such large primary flakes are difficult to agglomerate to form uniform and dense secondary balls, so it is difficult to form balls in the process, resulting in a relatively low tap density, which affects the processing performance of the material and further affects the volume energy density of the battery. Moreover, such large and thick primary particles have low activity during sintering, requiring a higher sintering temperature, and the primary particles after sintering are also large, which is not conducive to the electrochemical activity of the material.
[0005] It can be seen that the current industry's preparation method for lithium-rich manganese-based precursors leads to poor sphericity, low tap density, coarse primary particles, and uneven thickness of primary flaky particles, which is not conducive to increasing capacity. In order to inhibit the agglomeration of secondary balls and control the size and distribution of secondary balls, organic complexing agents are often added in the prior art, which increases the production cost and brings influence and burden to subsequent water treatment. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects existing in the prior art and provide a lithium-rich manganese-based precursor material and a preparation method thereof, which can effectively solve the above-mentioned problems existing in the prior art.
[0007] To achieve the above object, the technical solution of the present invention is to provide
[0008] A lithium-rich manganese-based precursor material, the chemical formula of its hydroxide is Ni x Mn (1-x) (OH)2, where 0<x≤0.5.
[0009] Furthermore, the particle size D50 of the secondary particles is 3-12 μm; the tap density is ≥1.40 g / cm 3 , with a specific surface area of 5-25m 2 / g.
[0010] Further, it comprises the following steps:
[0011] S1: dissolving soluble salts of nickel and manganese in water to prepare a nickel-manganese metal mixed salt solution, wherein the molar ratio x of nickel to manganese is in the range of 0<x≤0.5; and simultaneously preparing a sodium hydroxide solution and aqueous ammonia;
[0012] S2: adding water, ammonia water and sodium hydroxide solution into the synthesis equipment in sequence as the reaction start-up bottom solution;
[0013] S3: introduce nitrogen into the synthesis equipment, start stirring, control the speed, and raise the temperature of the reactor to 30-50°C and stabilize it;
[0014] S4: Under a nitrogen atmosphere, the nickel-manganese mixed salt solution, sodium hydroxide solution and ammonia solution described in S1 are pumped into the bottom liquid of the synthesis equipment, stirring is started, and the temperature, pH value and ammonia value during the reaction are controlled;
[0015] S5: Make the D50 of the reaction slurry reach the target value through the synthesis equipment;
[0016] S6: When the D50 of the reaction slurry reaches the target value, the reaction slurry is filtered and washed to obtain a washed filter cake;
[0017] S7: Dry the washed filter cake, and after the moisture content is qualified, sieve and demagnetize it in sequence to obtain a lithium-rich manganese-based precursor material product.
[0018] Furthermore, in step S1, the molar concentration of the metal mixed salt solution is 1.0 to 2.3 mol / L, the molar concentration of the sodium hydroxide solution is 1.0 to 12.0 mol / L, and the molar concentration of the ammonia water is 1.0 to 12.0 mol / L.
[0019] Furthermore, in step S2, the pH value of the startup base liquid is 10.0-13.0, and the ammonia concentration is 1.0 g / L-14.0 g / L;
[0020] In step S2, the stirring speed is 50-600 rpm and the reaction temperature is 35-70°C.
[0021] Furthermore, the synthesis equipment includes a kettle A (feeding reactor) and a kettle B (concentrating reactor), the kettle A (feeding reactor) is provided with an overflow valve and is connected to the kettle B (concentrating reactor), and the kettle B (concentrating reactor) is connected to the kettle A (feeding reactor) through a circulating pump.
[0022] Furthermore, in steps S2, S3 and S4, the synthesis equipment only involves reactor A (feed reactor).
[0023] Furthermore, in step S5, the specific operation steps are as follows:
[0024] When the liquid level of kettle A (feed reactor) reaches full, the overflow valve to kettle B (concentration reactor) opens. At this time, the slurry in kettle B keeps circulating with kettle A through the circulation pump;
[0025] When the B reactor is full, the concentration is started, the clear liquid is discharged, and the concentrated slurry is stored in the reactor;
[0026] When D50 reaches 8μm, kettle B continues to receive overflow material from kettle A, but the slurry in kettle B no longer returns to kettle A; when D50 of kettle A reaches 13.5μm, kettle A stops feeding and the slurries in kettles A and B are started to circulate; after circulating for 2h, the mixed particle size D50=10.0μm is tested, and then the slurries in kettles A and B are discharged into the aging tank.
[0027] Furthermore, in step S6, the specific operation steps are as follows:
[0028] After solid-liquid separation, the slurry in the aging tank is first washed with a prepared dilute alkali solution and then washed with pure water to obtain a washed filter cake;
[0029] Preferably, the concentration of the dilute alkali solution is 0.1-2.0 mol / L, and the temperature is 50-70°C; the temperature of the pure water is 50-70°C;
[0030] Preferably, after solid-liquid separation, the slurry in the aging tank is sequentially heated to 3 m 3 0.8mol / L of liquid caustic soda and 4m 3 Wash with pure water to obtain a washed filter cake;
[0031] Further, in step S7, the specific operation steps are as follows: drying the washed filter cake at 80-130° C. for 2-5 hours, heating to 100-150° C. for drying for 0.5-2 hours, and then sieving and demagnetizing in sequence to obtain a lithium-rich manganese-based precursor material product;
[0032] Preferably, the washed filter cake is dried at 80° C. for 4 h, then heated to 120° C. and dried for 0.5 h. After the moisture content is qualified, the filter cake is sieved and demagnetized to obtain a lithium-rich manganese-based precursor material product.
[0033] Furthermore, in step S4, the stirring speed is adjusted according to the growth of D50, specifically as follows: the speed is 300 rpm when starting the kettle, when the particle size is 5 μm, the speed is adjusted to 270 rpm, when the particle size is 7 μm, the speed is adjusted to 260 rpm, and when the particle size is 9 μm, the speed is adjusted to 250 rpm.
[0034] The advantages and beneficial effects of the present invention are:
[0035] (1) If the primary particles are too coarse, the secondary balls will be too compact, which will not only affect the precipitation of impurities such as Na and S, but also affect the processing performance of the material, which is not conducive to the sintering of the positive electrode material, resulting in low capacity and poor cycle performance. When the primary particles are flaky and the secondary balls are too loose, the tap density is low, which is not conducive to the increase of later production capacity. A lithium-rich manganese-based precursor material with uniform primary particles can be prepared through a specific synthesis process;
[0036] (2) The present invention does not require surfactants or crystal growth directing agents, has a simple preparation method, does not increase the burden of wastewater treatment, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a SEM image of Example 1 of the present invention;
[0038] Figure 2 is a SEM image of Example 2 of the present invention;
[0039] Figure 3 is a SEM image of Example 3 of the present invention;
[0040] Figure 4 This is the SEM image of Example 4 of the present invention. DETAILED DESCRIPTION
[0041] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0042] (I) Preparation of lithium-rich manganese-based precursor materials
[0043] Embodiment 1:
[0044] The present invention provides a method for preparing a lithium-rich manganese-based precursor material, comprising the following steps:
[0045] S1. NiSO4 and MnSO4 are prepared into a 2 mol / L nickel-manganese metal salt mixed solution according to a molar ratio of 30:70, and a sodium hydroxide solution with a concentration of 10.5 mol / L and an ammonia solution with a concentration of 7.5 mol / L are prepared;
[0046] S2, adding pure water, the ammonia water and the sodium hydroxide solution into the reaction kettle in sequence to form a start-up base liquid with a pH of 12.05 and an ammonia concentration of 4.30 g / L;
[0047] S3, introduce nitrogen into the reactor, start stirring, control the speed to 300 rpm, and raise the temperature of the reactor to 38° C. and stabilize it;
[0048] S4. The prepared nickel and manganese metal mixed salt solution, ammonia water and sodium hydroxide solution are sequentially added into the A kettle (feed reactor) using a metering pump, and the feeding reaction is started under the protection of nitrogen gas; during the reaction granulation, the temperature is controlled at 38°C, the ammonia value is 4.30 g / L, and the reaction is carried out at a pH value of 12.05 for 2 hours; after 2 hours, the reaction ammonia value is increased by 6.5 g / L, the temperature is increased to 50°C and stabilized, and the pH slowly decreases to 10.55.
[0049] S5. When the liquid level of kettle A (feeding reactor) reaches full, the overflow valve to kettle B (concentrating reactor) is opened. At this time, the slurry in kettle B keeps circulating with kettle A through the circulation pump. When kettle B is full, the concentration is started, the clear liquid is discharged, and the concentrated slurry is stored in the reactor. When D50 reaches 8μm, kettle B continues to receive the overflow material from kettle A, but the slurry in kettle B no longer returns to kettle A. When kettle A D50 reaches 13.5μm, kettle A stops feeding, and the slurry in kettles A and B is circulated. After circulating for 2h, the mixed particle size D50=10.0μm is tested. Then the slurry in kettles A and B is discharged into the aging tank.
[0050] S6, after solid-liquid separation, the slurry in the aging tank is heated to 60°C and then 3 0.8mol / L liquid caustic soda and 4m 3 Wash with pure water to obtain a washed filter cake.
[0051] S7. Dry the washed filter cake at 80° C. for 4 h, heat it to 120° C., and after the moisture content is qualified (moisture content < 0.6%), sieve it and demagnetize it to obtain a lithium-rich manganese-based precursor material product.
[0052] Embodiment 2:
[0053] The present invention provides a method for preparing a lithium-rich manganese-based precursor material, comprising the following steps:
[0054] S1. NiSO4 and MnSO4 are prepared into a 2 mol / L nickel-manganese metal salt mixed solution according to a molar ratio of 30:70, and a sodium hydroxide solution with a concentration of 10.5 mol / L and an ammonia solution with a concentration of 7.5 mol / L are prepared;
[0055] S2, adding pure water, the ammonia water and the sodium hydroxide solution into the reaction kettle in sequence to form a start-up base liquid with a pH of 12.05 and an ammonia concentration of 4.30 g / L;
[0056] S3, introduce nitrogen into the reactor, start stirring, control the speed to 300 rpm, and raise the temperature of the reactor to 38° C. and stabilize it;
[0057] S4. The prepared nickel and manganese metal mixed salt solution, ammonia water and sodium hydroxide solution are sequentially added into the A kettle (feed reactor) using a metering pump, and the feeding reaction is started under the protection of nitrogen gas; during the reaction granulation, the temperature is controlled at 38°C, the ammonia value is 4.30 g / L, and the reaction is carried out at a pH value of 12.05 for 2 hours; after 2 hours, the reaction ammonia value is increased by 6.5 g / L, the temperature is increased to 50°C and stabilized, and the pH slowly decreases to 10.55.
[0058] S5. When the liquid level of kettle A (feeding reactor) reaches full, the overflow valve to kettle B (concentration reactor) is opened. At this time, the slurry in kettle B is kept circulating with kettle A through the circulation pump. When kettle B is full, concentration is started, the clear liquid is discharged, and the concentrated slurry is stored in the reactor. Continue the reaction until D50 reaches 10.0μm, stop feeding, and then discharge the slurry in kettles A and B into the aging tank.
[0059] S6, after solid-liquid separation, the slurry in the aging tank is heated to 60°C and then 3 0.8mol / L liquid caustic soda and 4m 3 Wash with pure water to obtain a washed filter cake.
[0060] S7. Dry the washed filter cake at 80° C. for 4 h, heat it to 120° C., and after the moisture content is qualified (moisture content < 0.6%), sieve it and demagnetize it to obtain a lithium-rich manganese-based precursor material product.
[0061] Embodiment 3:
[0062] S1. NiSO4 and MnSO4 are prepared into a 2 mol / L nickel-manganese metal salt mixed solution according to a molar ratio of 30:70, and a sodium hydroxide solution with a concentration of 10.5 mol / L and an ammonia solution with a concentration of 7.5 mol / L are prepared;
[0063] S2, adding pure water, the ammonia water and the sodium hydroxide solution into the reaction kettle in sequence to form a start-up base liquid with a pH of 12.05 and an ammonia concentration of 4.30 g / L;
[0064] S3, introduce nitrogen into the reactor, start stirring, control the speed to 300 rpm, and raise the temperature of the reactor to 38° C. and stabilize it;
[0065] S4. The prepared nickel and manganese metal mixed salt solution, ammonia water and sodium hydroxide solution are sequentially added into the A kettle (feed reactor) using a metering pump, and the feeding reaction is started under the protection of nitrogen gas; during the reaction granulation, the temperature is controlled at 38°C, the ammonia value is 4.30 g / L, and the reaction is carried out at a pH value of 12.05 for 2 hours; after 2 hours, the reaction ammonia value is increased by 6.5 g / L, the temperature is increased to 50°C and stabilized, and the pH slowly decreases to 10.55.
[0066] S5. When the liquid level of kettle A (feeding reactor) reaches full, it overflows to the unqualified tank. When D50 of kettle A reaches 8μm, open the overflow valve to kettle B (concentration reactor), and switch from overflow to unqualified to kettle B. At the same time, the slurry in kettle B keeps circulating with kettle A through the circulation pump. When the liquid level of kettle B is full, start concentration, discharge the clear liquid, and store the concentrated slurry in the reactor. When D50 reaches 10.0μm, stop feeding, and then discharge the slurry in kettles A and B into the aging tank.
[0067] S6, after solid-liquid separation, the slurry in the aging tank is heated to 60°C and then 3 0.8mol / L liquid caustic soda and 4m 3 Wash with pure water to obtain a washed filter cake.
[0068] S7. Dry the washed filter cake at 80° C. for 4 h, heat it to 120° C., and after the moisture content is qualified (moisture content < 0.6%), sieve it and demagnetize it to obtain a lithium-rich manganese-based precursor material product.
[0069] Embodiment 4:
[0070] S1. NiSO4 and MnSO4 are prepared into a 2 mol / L nickel-manganese metal salt mixed solution according to a molar ratio of 30:70, and a sodium hydroxide solution with a concentration of 10.5 mol / L and an ammonia solution with a concentration of 7.5 mol / L are prepared;
[0071] S2, adding pure water, the ammonia water and the sodium hydroxide solution into the reaction kettle in sequence to form a start-up base liquid with a pH of 12.05 and an ammonia concentration of 4.30 g / L;
[0072] S3, introduce nitrogen into the reactor, start stirring, control the speed to 300 rpm, and raise the temperature of the reactor to 38° C. and stabilize it;
[0073] S4. The prepared nickel and manganese metal mixed salt solution, ammonia water and sodium hydroxide solution are sequentially added into the A kettle (feed reactor) using a metering pump, and the feeding reaction is started under the protection of nitrogen gas; during the reaction granulation, the temperature is controlled at 38°C, the ammonia value is 4.30 g / L, and the reaction is carried out at a pH value of 12.05 for 2 hours; after 2 hours, the reaction ammonia value is increased by 6.5 g / L, the temperature is increased to 50°C and stabilized, and the pH slowly decreases to 10.55.
[0074] S5. When the liquid level of kettle A (feeding reactor) reaches full, it overflows to the unqualified tank. When D50 of kettle A reaches 10.0 μm, kettle A stops feeding. Then the slurry in kettle A is discharged to the aging tank.
[0075] S6, after solid-liquid separation, the slurry in the aging tank is heated to 60°C and then 3 0.8mol / L liquid caustic soda and 4m 3 Wash with pure water to obtain a washed filter cake.
[0076] S7. Dry the washed filter cake at 80° C. for 4 h, heat it to 120° C., and after the moisture content is qualified (moisture content < 0.6%), sieve it and demagnetize it to obtain a lithium-rich manganese-based precursor material product.
[0077] (II) Performance test
[0078] The instrument parameters for determining the content of impurities Na and S are shown in the following table:
[0079] project equipment Sample size solvent Total wavelength S Agilent 0.4g Hydrochloric acid (10 mL) 50mL 182.562 Na Agilent 0.4g Hydrochloric acid (10 mL) 50mL 589.592
[0080] The instrument names, manufacturers and models used in SEM, BET and TD are shown in the following table:
[0081] project instrument Manufacturer model SEM Field Emission Scanning Electron Microscope Thermo Fisher Scientific Inc. Apreo2C BET Surface area meter Best Instrument Technology (Beijing) Co., Ltd. 3H-2000A TD Tap density tester Liaoning Instrument Research Institute Co., Ltd. ZS-203
[0082] The results of the experimental performance parameters of Examples 1-4 are shown in the following table:
[0083] D50(μm) Na(ppm) S(ppm) <![CDATA[BET(cm 2 / g)]]> <![CDATA[TD(g / cm 3 )]]> Example 1 10.03 122 1167 18.12 1.76 Example 2 9.92 198 1869 17.28 1.77 Example 3 9.89 118 1182 18.27 1.65 Example 4 10.04 113 1175 20.38 1.43
[0084] It can be seen from Examples 1-4 that step S5 determines different reaction systems (batch process, semi-continuous process, continuous process), which directly affects the morphology and physicochemical parameters of the product.
[0085] (III) Electrochemical performance test
[0086] The lithium-rich manganese-based precursor materials prepared in Examples 1-4 were mixed with LiOH at a molar ratio of Li:M (M=Ni+Mn)=1.65:1, and then placed in a muffle furnace and heated to 550°C for sintering for 6 hours. The materials were then heated to 900°C, 950°C, and 1000°C for sintering for 14 hours, and then naturally cooled to room temperature. The whole process was heated at 0.2 m 3 ·s -1 The sintered material is taken out from the muffle furnace, ground, sieved and dried.
[0087] The positive electrode material, acetylene black (SP) and polyvinylidene fluoride (PVDF) were weighed according to a mass ratio of 90:6:4, ground in a mortar for 30 minutes, and then an appropriate amount of N-methylpyrrolidone (NMP) was added and transferred to a homogenizer to make a slurry. Then, the slurry was coated on an aluminum foil and dried in a blast drying oven at 120°C for 30 minutes. The dried positive electrode sheet was rolled and punched to obtain a small disc with a radius of 0.6 cm. Then, the dried electrode sheet, diaphragm and other auxiliary tools were assembled into a button battery, with the lithium sheet as the negative electrode.
[0088] The prepared button half-cell was subjected to electrochemical performance tests at 2.75-4.30 V, and a 200-week cycle performance test at room temperature (25° C.). The results are shown in the following table.
[0089]
[0090] From the test performance, the positive electrode material prepared in Example 1 of the present invention exhibits relatively excellent electrochemical performance.
[0091] It can be seen from Examples 1-4 that step S5 determines different reaction systems (intermittent method, semi-continuous method, continuous method), which will directly affect the morphology, physicochemical parameters and electrochemical properties of the product. The main difference between Examples 1-4 is the morphology, which also largely determines its physicochemical parameters. When the tap density is close, the primary particles are slightly finer and can better exert the electrochemical properties. The primary particles are in a block shape and are too thick and dense, which is not conducive to the processing of the material and affects the electrochemical performance; and the primary particles are too sparse and are not conducive to the increase of production.
[0092] The present invention can prepare a lithium-rich manganese-based precursor material with uniform primary particles through a specific synthesis process; the present invention does not require a surfactant or a crystal growth directing agent, the preparation method is simple, does not increase the burden of wastewater treatment, and is suitable for industrial production.
[0093] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A lithium-rich manganese-based precursor material, characterized in that: The chemical formula of its hydroxide is Ni x Mn (1-x) (OH)2, where 0<x≤0.
5.
2. The lithium-rich manganese-based precursor material according to claim 1, characterized in that: The particle size D50 of secondary particles is 3-12μm; the tap density is ≥1.40g / cm 3 , with a specific surface area of 5-25m 2 / g.
3. A method for preparing a lithium-rich manganese-based precursor material as claimed in claim 1, characterized in that: It includes the following steps: S1: dissolving soluble salts of nickel and manganese in water to prepare a nickel-manganese metal mixed salt solution, wherein the molar ratio x of nickel to manganese is in the range of 0<x≤0.5; and simultaneously preparing a sodium hydroxide solution and aqueous ammonia; S2: adding water, ammonia water and sodium hydroxide solution into the synthesis equipment in sequence as the reaction start-up bottom solution; S3: introduce nitrogen into the synthesis equipment, start stirring, control the speed, and raise the temperature of the reactor to 30-50°C and stabilize it; S4: Under a nitrogen atmosphere, the nickel-manganese mixed salt solution, sodium hydroxide solution and ammonia solution described in S1 are pumped into the bottom liquid of the synthesis equipment, stirring is started, and the temperature, pH value and ammonia value during the reaction are controlled; S5: Make the D50 of the reaction slurry reach the target value through the synthesis equipment; S6: When the D50 of the reaction slurry reaches the target value, the reaction slurry is filtered and washed to obtain a washed filter cake; S7: Dry the washed filter cake, and after the moisture content is qualified, sieve and demagnetize it in sequence to obtain a lithium-rich manganese-based precursor material product.
4. The method for preparing a lithium-rich manganese-based precursor material according to claim 3, characterized in that: In step S1, the molar concentration of the metal mixed salt solution is 1.0-2.3 mol / L, the molar concentration of the sodium hydroxide solution is 1.0-12.0 mol / L, and the molar concentration of the ammonia water is 1.0-12.0 mol / L.
5. The method for preparing a lithium-rich manganese-based precursor material according to claim 3, characterized in that: In step S2, the pH value of the startup base liquid is 10.0-13.0, and the ammonia concentration is 1.0 g / L-14.0 g / L; In step S2, the stirring speed is 50-600 rpm and the reaction temperature is 35-70°C.
6. The method for preparing a lithium-rich manganese-based precursor material according to claim 3, characterized in that: The synthesis equipment comprises an A kettle (feeding reactor) and a B kettle (concentrating reactor). The A kettle (feeding reactor) is provided with an overflow valve and is connected to the B kettle (concentrating reactor). The B kettle (concentrating reactor) is connected to the A kettle (feeding reactor) through a circulation pump.
7. The method for preparing a lithium-rich manganese-based precursor material according to claim 6, characterized in that: In steps S2, S3 and S4, the synthesis equipment only involves reactor A (feed reactor).
8. The method for preparing a lithium-rich manganese-based precursor material according to claim 6, characterized in that: In step S5, the specific operation steps are as follows: When the liquid level of kettle A (feed reactor) reaches full, the overflow valve to kettle B (concentration reactor) opens. At this time, the slurry in kettle B keeps circulating with kettle A through the circulation pump; When the B reactor is full, the concentration is started, the clear liquid is discharged, and the concentrated slurry is stored in the reactor; When D50 reaches 8μm, kettle B continues to receive overflow material from kettle A, but the slurry in kettle B no longer returns to kettle A; when D50 of kettle A reaches 13.5μm, kettle A stops feeding and the slurries in kettles A and B are started to circulate; after circulating for 2h, the mixed particle size D50=10.0μm is tested, and then the slurries in kettles A and B are discharged into the aging tank.
9. The method for preparing a lithium-rich manganese-based precursor material according to claim 8, characterized in that: In step S6, the specific operation steps are as follows: After solid-liquid separation, the slurry in the aging tank is first washed with a prepared dilute alkali solution and then washed with pure water to obtain a washed filter cake.
10. The method for preparing a lithium-rich manganese-based precursor material according to claim 8, characterized in that: In step S7, the specific operation steps are as follows: drying the washed filter cake at 80-130° C. for 2-5 hours, heating to 100-150° C. for drying for 0.5-2 hours, and then sieving and demagnetizing to obtain a lithium-rich manganese-based precursor material product.