Sodium electric layered precursor with low sodium and sulfur content as well as preparation method and application of sodium electric layered precursor
By adsorbing carbonate ions in the sodium-electric layered precursor through the composite solution of sodium hydroxide and carbonate, replacing sulfate, solving the problem of removing sodium-sulfur impurities, realizing the preparation of low-content sodium-electric layered precursors, and improving the Battery cycle performance and simplifies the preparation process.
Patent Information
- Application Number
- CN202411070240.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing sodium-sulfur impurities are difficult to effectively remove in sodium-electric layered precursors, resulting in a decrease in battery capacity and cycling performance. The existing methods are complex and costly.
Using a composite solution composed of sodium hydroxide and carbonate, the hydroxyl band on the surface of the protonated hydroxide is positively charged, and carbonate ions are adsorbed to replace sulfate, reducing the sulfur content in the precursor, and carbonate is used when preparing the positive electrode material. Ion pyrolysis is made into CO2 to avoid the introduction of new impurities.
The sodium and sulfur content in the sodium-electric layered precursor was successfully reduced, so that it reached Na≤200ppm and S≤1300ppm, which improved the cycle stability of the positive electrode material and avoided additional washing steps.
Smart Images

Figure CN118978193A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium batteries, and relates to a sodium battery precursor and a preparation method and application thereof, and in particular to a sodium battery layered precursor with low sodium and sulfur content and a preparation method and application thereof. Background Art
[0002] Layered sodium-ion battery materials have become an excellent choice for next-generation battery materials due to their high cost-effectiveness, but sodium-sulfur impurities can have a negative impact on the capacity and cycle performance of the battery.
[0003] The main source of sodium sulfur impurities is the layered hydroxide precursor, which can act as an anion adsorbent to adsorb SO 4 2- , so in the process of preparing the precursor SO 4 2- It is easily adsorbed between primary grain layers and / or on the surface, causing excessive sodium and sulfur content in the precursor.
[0004] At present, sulfur removal mainly adopts two ways: post-washing and removal during the reaction. For example, the method disclosed in CN112234187A adds formamide molecules during the washing process at room temperature to increase the interlamellar spacing of the precursor through the molecular polarity, thereby reducing the Na + 、SO 4 2- However, the method of adding surfactants for washing during post-treatment can only wash away impurities on the surface of large-particle precursors, but cannot wash away particles inside the precursors; moreover, washing with organic surfactants is a complex and costly process.
[0005] The method disclosed in CN113683130A prepares precursor particles with radial cracks by controlling the pH drop. However, during the post-processing process, the positive electrode material is prone to intergranular cracks, resulting in the formation of a solid electrolyte interface (SEI) film when the battery is cycled for a long time at a high cut-off voltage, showing a rapid decay of the battery cycle capacity.
[0006] To this end, it is necessary to provide a sodium-ion battery layered precursor with low sodium and sulfur content, which can reduce the sodium and sulfur content in the precursor and ensure the cycle stability of the positive electrode material of the sodium ion battery, and a preparation method and application thereof. Summary of the invention
[0007] The purpose of the present invention is to provide a sodium layered precursor with low sodium and sulfur content and a preparation method and application thereof. The preparation method uses a composite solution composed of sodium hydroxide and carbonate to reduce the sulfur content in the sodium layered precursor, so that Na≤200ppm and S≤1300ppm; and when the obtained sodium layered precursor is used to prepare a positive electrode material, carbonate ions will be pyrolyzed into CO 2 Released, avoiding the introduction of new impurities and eliminating the need for washing with carbonates.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0010] The sulfate solution, the composite solution and the complexing agent solution are mixed in parallel in the bottom liquid, and sequentially undergo nucleation reaction, crystal growth reaction and aging, solid-liquid separation, and then drying to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content;
[0011] The solute in the composite solution includes a precipitant and an additive in a molar ratio of 100:(0.5-1), for example, 100:0.5, 100:0.6, 100:0.8, 100:0.9 or 100:1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0012] The precipitant includes sodium hydroxide;
[0013] The additive includes a carbonate.
[0014] The preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate. The hydroxyl groups on the surface of the layered hydroxide are protonated and the whole layered hydroxide is positively charged. The anionic carbonate can be adsorbed to compete with the negatively charged sulfate and replace a part of the sulfate position, thereby achieving the purpose of reducing the interlayer sulfur content. The preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate, which reduces the sulfur content in the sodium-electrode layered precursor, making Na≤200ppm and S≤1300ppm; and when preparing the positive electrode material, the carbonate ions will be pyrolyzed into CO 2 Released, avoiding the introduction of new impurities and eliminating the need for washing with carbonates.
[0015] Preferably, the carbonate comprises any one of sodium carbonate, potassium carbonate or ammonium carbonate or a combination of at least two thereof, typical but non-limiting combinations comprising a combination of sodium carbonate and potassium carbonate, a combination of sodium carbonate and ammonium carbonate, a combination of potassium carbonate and ammonium carbonate, or a combination of sodium carbonate, potassium carbonate and ammonium carbonate.
[0016] Preferably, the concentration of sodium hydroxide in the composite solution is 8-12 mol / L, for example, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0017] Preferably, the pH value of the nucleation reaction is 11-12, for example, 11, 11.5 or 12, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Preferably, the concentration of the complexing agent during the nucleation reaction is 0.1-0.3 mol / L, for example, 0.1 mol / L, 0.2 mol / L or 0.3 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the temperature of the nucleation reaction is 60-70°C, for example, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the target particle size D50 of the nucleation reaction reaches 3.3-3.8 μm, for example, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm or 3.8 μm, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0021] Preferably, the nucleation reaction is carried out under a stirring condition of 750-850 rpm, for example, 750 rpm, 780 rpm, 800 rpm, 820 rpm or 850 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the pH value of the crystal growth reaction is 8-11, for example, 8, 9, 10 or 11, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the concentration of the complexing agent during the crystal growth reaction is 0.1-0.3 mol / L, for example, 0.1 mol / L, 0.2 mol / L or 0.3 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the temperature of the crystal growth reaction is 60-70°C, for example, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the target particle size of the crystal growth reaction is D50 reaching 14 μm or more, for example, it can be 14 μm, 14.5 μm, 15 μm, 15.5 μm or 16 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the crystal growth reaction is carried out under a stirring condition of 750-850 rpm, for example, 750 rpm, 780 rpm, 800 rpm, 820 rpm or 850 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the pH value of the aging is 10-12, for example, it can be 10, 10.5, 11 or 11.5 or 12, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0028] Preferably, the aging temperature is 40-80°C, for example, 40°C, 50°C, 60°C, 70°C or 80°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the total alkalinity of the aging is 10-40 g / L, for example, 10 g / L, 20 g / L, 30 g / L or 40 g / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] During the aging process of the present invention, the pH value and the total alkalinity are adjusted by adding sodium hydroxide and carbonate.
[0031] Preferably, the aging time is more than 8 hours, for example, it can be 8 hours, 9 hours, 10 hours, 11 hours or 12 hours, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0032] Preferably, the aging is carried out under stirring conditions of 200-600 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm or 600 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the base liquid comprises water, sodium hydroxide and a complexing agent.
[0034] Preferably, the pH value of the base solution is 11-12, for example, it can be 11, 11.5 or 12, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0035] Preferably, the concentration of the complexing agent in the base solution is 0.1-0.3 mol / L, for example, 0.1 mol / L, 0.2 mol / L or 0.3 mol / L, but is not limited to the listed values, and other values not listed in the numerical range are also applicable;
[0036] Preferably, the temperature of the base liquid is 60-70°C, for example, 60°C, 62°C, 65°C, 68°C or 70°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] As a preferred technical solution of the preparation method described in the first aspect, the preparation method comprises the following steps:
[0038] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution consisting of water, sodium hydroxide and a complexing agent to sequentially perform a nucleation reaction and a crystal growth reaction;
[0039] The sulfate concentration in the sulfate solution is 80-120 g / L; the sulfate includes nickel sulfate, iron sulfate and manganese sulfate;
[0040] The solute in the composite solution includes a precipitant and an additive in a molar ratio of 100:(0.5-1);
[0041] The precipitant includes sodium hydroxide;
[0042] The additive includes carbonate; the carbonate includes any one of sodium carbonate, potassium carbonate or ammonium carbonate or a combination of at least two;
[0043] The concentration of sodium hydroxide in the composite solution is 8-12 mol / L;
[0044] The concentration of the complexing agent solution is 7-11 mol / L;
[0045] The complexing agent in the complexing agent solution and the base solution independently comprises any one of oxalic acid, citric acid, ascorbic acid or ammonia water or a combination of at least two thereof;
[0046] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 200-600 rpm, and the mixture is aged for more than 8 hours under protective atmosphere conditions; the aging temperature is 40-80° C., the pH value during aging is 10-12, and the total alkalinity is 10-40 g / L;
[0047] (3) solid-liquid separation, washing with water for 2-3 times, and then drying at 80-120° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0048] In a second aspect, the present invention provides a sodium-electrolyte layered precursor with low sodium and sulfur content, and the sodium-electrolyte layered precursor with low sodium and sulfur content is prepared by the preparation method described in the first aspect.
[0049] In the third aspect, the present invention provides a positive electrode material, characterized in that the positive electrode material is prepared from a sodium-electrolyte layered precursor with low sodium and sulfur content obtained by the preparation method described in the first aspect of claim, or the positive electrode material is prepared from the sodium-electrolyte layered precursor with low sodium and sulfur content described in the second aspect.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] The preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate. The hydroxyl groups on the surface of the layered hydroxide are protonated and are positively charged as a whole. The anionic carbonate can be adsorbed to compete with the negatively charged sulfate and replace a part of the sulfate position, thereby achieving the purpose of reducing the interlayer sulfur content. The preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate, which reduces the sulfur content in the sodium-electrode layered precursor, making Na≤200PPm and S≤1300ppm; and when preparing the positive electrode material, the carbonate ions will be pyrolyzed into CO 2 Released, avoiding the introduction of new impurities and eliminating the need for washing with carbonates. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in Example 1;
[0053] Figure 2 This is a SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in Example 2;
[0054] Figure 3 This is a SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in Example 3;
[0055] Figure 4 This is the SEM image of the sodium electrode layered precursor obtained in Comparative Example 1. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0057] Example 1
[0058] This embodiment provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0059] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to sequentially perform a nucleation reaction and a crystal growth reaction;
[0060] The sulfate concentration in the sulfate solution is 80 g / L; the sulfate comprises nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0061] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:1;
[0062] The concentration of sodium hydroxide in the composite solution is 10 mol / L;
[0063] The complexing agent solution is ammonia water with a concentration of 8 mol / L;
[0064] The pH value of the nucleation reaction is 11.5, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65°C, the target particle size D50 reaches 3.5 μm, and the nucleation reaction is carried out under stirring conditions of 800 rpm;
[0065] The pH value of the crystal growth reaction is 10, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65° C., the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 800 rpm;
[0066] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 400 rpm and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 60° C., the pH value during aging is 11, and the total alkalinity is 25 g / L;
[0067] (3) solid-liquid separation, washing with water for three times, and then drying at 100° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0068] The SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in this example is as follows: Figure 1 shown.
[0069] Example 2
[0070] This embodiment provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0071] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to sequentially perform a nucleation reaction and a crystal growth reaction;
[0072] The sulfate concentration in the sulfate solution is 80 g / L; the sulfate comprises nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0073] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:0.5;
[0074] The concentration of sodium hydroxide in the composite solution is 10 mol / L;
[0075] The complexing agent solution is ammonia water with a concentration of 8 mol / L;
[0076] The pH value of the nucleation reaction is 11.5, the concentration of the complexing agent is 0.1 mol / L, the temperature is 65°C, the target particle size D50 reaches 3.5 μm, and the nucleation reaction is carried out under stirring conditions of 800 rpm;
[0077] The pH value of the crystal growth reaction is 10, the concentration of the complexing agent is 0.1 mol / L, the temperature is 65° C., the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 800 rpm;
[0078] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 400 rpm and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 60° C., the pH value during aging is 11, and the total alkalinity is 25 g / L;
[0079] (3) solid-liquid separation, washing with water for three times, and then drying at 100° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0080] The SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in this example is as follows: Figure 2 shown.
[0081] Example 3
[0082] This embodiment provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0083] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to sequentially perform a nucleation reaction and a crystal growth reaction;
[0084] The sulfate concentration in the sulfate solution is 100 g / L; the sulfate includes nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0085] The solute in the composite solution includes sodium hydroxide and ammonium carbonate in a molar ratio of 100:1;
[0086] The concentration of sodium hydroxide in the composite solution is 10 mol / L;
[0087] The complexing agent solution is ammonia water with a concentration of 8 mol / L;
[0088] The pH value of the nucleation reaction is 11.5, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65°C, the target particle size D50 reaches 3.5 μm, and the nucleation reaction is carried out under stirring conditions of 800 rpm;
[0089] The pH value of the crystal growth reaction is 10, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65° C., the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 800 rpm;
[0090] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 400 rpm and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 60° C., the pH value during aging is 11, and the total alkalinity is 25 g / L;
[0091] (3) solid-liquid separation, washing with water for three times, and then drying at 100° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0092] The SEM image of the sodium-electrolyte layered precursor with low sodium and sulfur content obtained in this example is as follows: Figure 3 shown.
[0093] Example 4
[0094] This embodiment provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0095] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to sequentially perform a nucleation reaction and a crystal growth reaction;
[0096] The sulfate concentration in the sulfate solution is 80 g / L; the sulfate comprises nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0097] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:1;
[0098] The concentration of sodium hydroxide in the composite solution is 8 mol / L;
[0099] The complexing agent solution is ammonia water with a concentration of 7 mol / L;
[0100] The pH value of the nucleation reaction is 11, the concentration of the complexing agent is 0.1 mol / L, the temperature is 60°C, the target particle size D50 reaches 3.3 μm, and the nucleation reaction is carried out under stirring conditions of 750 rpm;
[0101] The pH value of the crystal growth reaction is 8, the concentration of the complexing agent is 0.1 mol / L, the temperature is 60° C., the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 750 rpm;
[0102] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 200 rpm, and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 40° C., the pH value during aging is 10, and the total alkalinity is 10 g / L;
[0103] (3) solid-liquid separation, washing with water for three times, and then drying at 80° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0104] Example 5
[0105] This embodiment provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, the preparation method comprising the following steps:
[0106] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to sequentially perform a nucleation reaction and a crystal growth reaction;
[0107] The sulfate concentration in the sulfate solution is 120 g / L; the sulfate comprises nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0108] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:1;
[0109] The concentration of sodium hydroxide in the composite solution is 12 mol / L;
[0110] The complexing agent solution is ammonia water with a concentration of 11 mol / L;
[0111] The pH value of the nucleation reaction is 12, the concentration of the complexing agent is 0.3 mol / L, the temperature is 70°C, the target particle size D50 reaches 3.8 μm, and the nucleation reaction is carried out under stirring conditions of 850 rpm;
[0112] The pH value of the crystal growth reaction is 11, the concentration of the complexing agent is 0.3 mol / L, the temperature is 70°C, the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 850 rpm;
[0113] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 600 rpm, and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 80° C., the pH value during aging is 12, and the total alkalinity is 40 g / L;
[0114] (3) solid-liquid separation, washing with water for three times, and then drying at 120° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0115] Comparative Example 1
[0116] This comparative example provides a method for preparing a sodium electric layered precursor, which is the same as Example 1 except that the molar amount of sodium carbonate in the composite solution is replaced by sodium hydroxide.
[0117] The SEM image of the sodium electrode layered precursor obtained in this comparative example is as follows Figure 4 shown.
[0118] Comparative Example 2
[0119] This comparative example provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, and the preparation method comprises the following steps:
[0120] (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution composed of water, sodium hydroxide and ammonia water to perform a nucleation reaction;
[0121] The sulfate concentration in the sulfate solution is 100 g / L; the sulfate includes nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0122] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:1;
[0123] The concentration of sodium hydroxide in the composite solution is 10 mol / L;
[0124] The complexing agent solution is ammonia water with a concentration of 8 mol / L;
[0125] The pH value of the nucleation reaction is 11.5, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65°C, the target particle size D50 reaches 15 μm, and the nucleation reaction is carried out under stirring conditions of 800 rpm;
[0126] (2) After the nucleation reaction is completed, the stirring speed is reduced to 400 rpm, and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 60° C., the pH value during aging is 11, and the total alkalinity is 25 g / L;
[0127] (3) solid-liquid separation, washing with water for three times, and then drying at 100° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0128] Comparative Example 3
[0129] This comparative example provides a method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, and the preparation method comprises the following steps:
[0130] (1) mixing a sulfate solution, a composite solution and a complexing agent solution in parallel in a base solution composed of water, sodium hydroxide and ammonia water to carry out a crystal growth reaction;
[0131] The sulfate concentration in the sulfate solution is 100 g / L; the sulfate includes nickel sulfate, iron sulfate and manganese sulfate in a molar ratio of 1:1:1;
[0132] The solute in the composite solution includes sodium hydroxide and sodium carbonate in a molar ratio of 100:1;
[0133] The concentration of sodium hydroxide in the composite solution is 10 mol / L;
[0134] The complexing agent solution is ammonia water with a concentration of 8 mol / L;
[0135] The pH value of the crystal growth reaction is 10, the concentration of the complexing agent is 0.2 mol / L, the temperature is 65° C., the target particle size D50 reaches 15 μm, and the crystal growth reaction is carried out under stirring conditions of 800 rpm;
[0136] (2) After the crystal growth reaction is completed, the stirring speed is reduced to 400 rpm and the mixture is aged for 8 h under a nitrogen atmosphere; the aging temperature is 60° C., the pH value during aging is 11, and the total alkalinity is 25 g / L;
[0137] (3) solid-liquid separation, washing with water for three times, and then drying at 100° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
[0138] Performance Characterization
[0139] The Na content and S content in the sodium-ion layered precursors obtained in the above examples and comparative examples were measured by inductively coupled plasma optical emission spectroscopy (ICP-OES), and the results are shown in Table 1.
[0140] Table 1
[0141] Na content (ppm) S content (ppm) Example 1 157 1188 Example 2 99 1054 Example 3 146 1203 Example 4 142 1197 Example 5 143 1084 Comparative Example 1 398 2459 Comparative Example 2 256 1972 Comparative Example 3 211 1620
[0142] In summary, the preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate. The hydroxyl groups on the surface of the layered hydroxide are protonated and are positively charged as a whole, and can adsorb anionic carbonates to compete with negatively charged sulfates and replace a portion of sulfate positions, thereby achieving the purpose of reducing the interlayer sulfur content. The preparation method provided by the present invention uses a composite solution composed of sodium hydroxide and carbonate, which reduces the sulfur content in the sodium-electrode layered precursor, making Na≤200ppm and S≤1300ppm; and when preparing the positive electrode material, the carbonate ions will be pyrolyzed into CO 2Released, avoiding the introduction of new impurities and eliminating the need for washing with carbonates.
[0143] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a sodium-electrolyte layered precursor with low sodium and sulfur content, characterized in that: The preparation method comprises the following steps: The sulfate solution, the composite solution and the complexing agent solution are mixed in parallel in the bottom liquid, and sequentially undergo nucleation reaction, crystal growth reaction and aging, solid-liquid separation, and then drying to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content; The solute in the composite solution includes a precipitant and an additive in a molar ratio of 100:(0.5-1); The precipitant includes sodium hydroxide; The additive includes a carbonate.
2. The preparation method according to claim 1, characterized in that: The carbonate includes any one of sodium carbonate, potassium carbonate or ammonium carbonate, or a combination of at least two of them.
3. The preparation method according to claim 1 or 2, characterized in that: The concentration of sodium hydroxide in the composite solution is 8-12 mol / L.
4. The preparation method according to any one of claims 1 to 3, characterized in that The pH value of the nucleation reaction is 11-12; Preferably, the concentration of the complexing agent during the nucleation reaction is 0.1-0.3 mol / L; Preferably, the temperature of the nucleation reaction is 60-70°C; Preferably, the target particle size of the nucleation reaction is D50 reaching 3.3-3.8 μm; Preferably, the nucleation reaction is carried out under stirring conditions of 750-850 rpm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The pH value of the crystal growth reaction is 8-11; Preferably, the concentration of the complexing agent during the crystal growth reaction is 0.1-0.3 mol / L; Preferably, the temperature of the crystal growth reaction is 60-70°C; Preferably, the target particle size of the crystal growth reaction is D50 reaching 14 μm or more; Preferably, the crystal growth reaction is carried out under stirring conditions of 750-850 rpm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The pH value of the aging is 10-12; Preferably, the aging temperature is 40-80°C; Preferably, the total alkalinity of the aging is 10-40 g / L; Preferably, the aging time is more than 8 hours; Preferably, the aging is carried out under stirring conditions of 200-600 rpm.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The base liquid includes water, sodium hydroxide and a complexing agent; Preferably, the pH value of the base liquid is 11-12; Preferably, the concentration of the complexing agent in the base solution is 0.1-0.3 mol / L; Preferably, the temperature of the base liquid is 60-70°C.
8. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) a sulfate solution, a composite solution and a complexing agent solution are mixed in parallel in a base solution consisting of water, sodium hydroxide and a complexing agent to sequentially perform a nucleation reaction and a crystal growth reaction; The sulfate concentration in the sulfate solution is 80-120 g / L; the sulfate includes nickel sulfate, iron sulfate and manganese sulfate; The solute in the composite solution includes a precipitant and an additive in a molar ratio of 100:(0.5-1); The precipitant includes sodium hydroxide; The additive includes carbonate; the carbonate includes any one of sodium carbonate, potassium carbonate or ammonium carbonate or a combination of at least two; The concentration of sodium hydroxide in the composite solution is 8-12 mol / L; The concentration of the complexing agent solution is 7-11 mol / L; The complexing agent in the complexing agent solution and the base solution independently comprises any one of oxalic acid, citric acid, ascorbic acid or ammonia water or a combination of at least two thereof; (2) After the crystal growth reaction is completed, the stirring speed is reduced to 200-600 rpm, and the mixture is aged for more than 8 hours under protective atmosphere conditions; the aging temperature is 40-80° C., the pH value during aging is 10-12, and the total alkalinity is 10-40 g / L; (3) solid-liquid separation, washing with water for 2-3 times, and then drying at 80-120° C. to obtain the sodium-electrolyte layered precursor with low sodium and sulfur content.
9. A sodium-electrolyte layered precursor with low sodium and sulfur content, characterized in that: The sodium-electrolyte layered precursor with low sodium and sulfur content is prepared by the preparation method described in any one of claims 1 to 8.
10. A positive electrode material, characterized in that: The positive electrode material is prepared from a sodium-electrolyte layered precursor with low sodium and sulfur content obtained by the preparation method described in any one of claims 1 to 8, or the positive electrode material is prepared from a sodium-electrolyte layered precursor with low sodium and sulfur content described in claim 9.
Citation Information
Cited By
Preparation method of nickel-iron-manganese sodium ion battery precursor
CN119612623A
Low-sodium-sulfur basic carbonate small-particle precursor as well as preparation method and application thereof
CN121627077A