Ceramic wine bottle inner glaze and preparation method thereof

By using quartzite, potassium feldspar, calcite, talc and metal composite powder in the inner glaze of ceramic wine bottles, the poor adhesion and cracks of the glaze surface in the inner glaze of ceramic wine bottles are solved, forming a high adhesion and wear-resistant inner glaze. layer to ensure the quality of the wine and anti-leakage effect.

CN118978336AActive Publication Date: 2024-11-19JIANGSU YIXIANG CERAMIC TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411087352.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The glaze surface in the ceramic wine bottle has poor adhesion, uneven glaze layer and dry cracks, which leads to the inability to effectively prevent the leakage of the wine and affect the quality of the wine.

Method used

The inner glaze of ceramic wine bottles using quartzite, potassium feldspar, calcite, talc, metal composite powder and colorants is formed through specific mixing and sintering processes to form an inner glaze layer with high adhesion, high strength and wear resistance. Reduce bubble generation and increase density and gloss.

Benefits of technology

It realizes uniform and smooth glaze in ceramic wine bottles, strong adhesion and no cracks, effectively preventing the leakage of the wine and maintaining the freshness and taste of the wine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978336A_ABST
    Figure CN118978336A_ABST
Patent Text Reader

Abstract

The invention relates to a ceramic wine bottle inner glaze and a preparation method thereof, and the ceramic wine bottle inner glaze comprises the following components in parts by weight: 30-50 parts of quartz stone, 25-50 parts of potassium feldspar, 16-32 parts of calcite, 12-24 parts of talc, 8-16 parts of metal composite powder, 5-10 parts of a coloring agent, 1.2-3.6 parts of a tackifier and 30-40 parts of deionized water. The internal glaze capable of being used for the ceramic wine bottle is prepared, the internal glaze comprises main raw materials such as quartzite, potassium feldspar, calcite and talc and further comprises metal composite powder as a reinforcing material, and part of a coloring agent is added. The prepared inner glaze is uniform and smooth on the ceramic wine bottle, is high in adhesive force and strength, is not easy to crack, and can well prevent leakage of wine liquid and maintain freshness and taste of the wine liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic materials, and in particular to an inner glaze of a ceramic wine bottle and a preparation method thereof. Background Art

[0002] Traditional wine bottles are generally made of glass, which has the defects of high firing temperature and high energy consumption. Therefore, ceramic wine bottles are often used to package wine. Ceramic wine bottles have unique advantages. On the one hand, the opaque nature of ceramic wine bottles can prevent light from causing chemical reactions in liquor and ensure the quality of liquor. On the other hand, ceramic wine bottles are slower than glass wine bottles in heat conduction, which can ensure the temperature of liquor and prevent liquor from deteriorating in low or high temperature environments. In addition, ceramic wine bottles also have the characteristics of aging and diverse appearance decoration. They are not only used as wine containers, but also as decorations. In particular, the unique decorative effect formed by glazing cannot be reflected in glass wine bottles. Therefore, ceramic wine bottles gradually replace glass wine bottles and become the main container for packaging wine. They are increasingly valued in the packaging of alcoholic beverages, especially liquor. A large number of famous wines use ceramic wine bottles as containers.

[0003] There are two types of ceramic wine bottles on the market: inner glaze and unglazed. Unglazed wine bottles are fired directly without coating the inner wall, and the wine is in direct contact with the wall. Inner glaze is to apply a layer of paint on the inner wall of the wine jar, and then fire it at high temperature to form a transparent glass coating, which plays a role in protecting the inner wall and preventing the wine from leaking. The inner glaze treatment can ensure that the inner wall of the wine jar is smooth, sterile, corrosion-resistant, and easy to clean, which can maintain the freshness and taste of the wine, while preventing the wine from leaking and oxidizing.

[0004] However, the inner glaze surface of ceramic wine bottles currently has problems such as poor glaze adhesion, uneven glaze layer, and easy cracking after drying. As a result, the inner glaze surface not only fails to prevent wine leakage, but also some glaze falls into the wine, affecting the quality of the wine. Summary of the invention

[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide a ceramic wine bottle inner glaze and a preparation method thereof.

[0006] The purpose of the present invention is achieved by the following technical solutions: In a first aspect, the present invention provides a ceramic wine bottle inner glaze, calculated by weight, comprising: 30-50 parts of quartz stone, 25-50 parts of potassium feldspar, 16-32 parts of calcite, 12-24 parts of talc, 8-16 parts of metal composite powder, 5-10 parts of colorant, 1.2-3.6 parts of tackifier and 30-40 parts of deionized water.

[0007] Preferably, the purity of the quartz stone is higher than 99.9% and the particle size is 10-20 μm.

[0008] Preferably, the purity of the potassium feldspar is higher than 99% and the particle size is 10-20 μm.

[0009] Preferably, the purity of the calcite is higher than 99.5% and the particle size is 10-20 μm.

[0010] Preferably, the purity of the talc is higher than 99% and the particle size is 10-20 μm.

[0011] Preferably, the colorant is one or a combination of titanium dioxide, magnesium oxide, iron oxide, and calcium borate.

[0012] Preferably, the viscosity enhancer is one or a combination of sodium carboxymethyl cellulose, sodium hydroxyethyl cellulose, polyacrylamide, and polyvinyl alcohol.

[0013] Preferably, the method for preparing the metal composite powder comprises: S1. Mix iridium trichloride (IrCl3) and scandium trichloride (ScCl3) in deionized water, stir thoroughly until uniform, then drop ammonia water, stir for 5-10 hours in an ice water bath, then warm to room temperature, continue stirring for 1-2 hours, filter out the precipitate, wash with water until the washing liquid is neutral, and vacuum dry to obtain a composite complex; S2, mixing the composite complex and tricalcium phosphate (Ca3(PO4)2) into a ball mill, and performing ball milling treatment under inert protection to obtain a composite product; S3. Sintering the composite product in a muffle furnace to obtain a metal composite powder.

[0014] More preferably, in S1, the mass volume ratio of iridium trichloride, scandium trichloride and deionized water is (0.3-0.6) g: (0.15-0.3) g: (10-20) mL.

[0015] More preferably, in S1, the mass fraction of ammonia water is 20%-30%, and the added amount is 10%-20% of the volume of deionized water.

[0016] More preferably, in S2, the mass ratio of the composite complex to tricalcium phosphate is 1:2.3-4.6.

[0017] More preferably, in S2, the ball milling speed is 350-450 r / min, the ball milling time is 3-6 h, and the ball-to-material ratio is 6-10:1.

[0018] More preferably, in S3, the sintering temperature is 400-500° C., and the sintering time is 2-4 hours.

[0019] In a second aspect, the present invention provides a method for preparing the inner glaze of a ceramic wine bottle, comprising the following steps: The first step is to weigh the thickener and deionized water according to the weight ratio, and mix them thoroughly to obtain a dispersion; The second step is to weigh quartz, potassium feldspar, calcite, talc, metal composite powder and colorant according to weight parts and add them into the dispersion liquid of the first step to obtain a raw material mixed liquid; The third step is to fully mix the raw material mixture in the second step until it is uniform, thereby obtaining the inner glaze slurry; The fourth step is to glaze the inner surface of the ceramic wine bottle blank with the inner glaze slurry, and then bake it in a high-temperature furnace to form the inner glaze of the ceramic wine bottle.

[0020] Preferably, the calcination process is: firstly heating to 700-800°C at a rate of 2-4°C / min, then heating to 850-950°C at a rate of 1-2°C / min, keeping the temperature for 20-30 minutes, and then cooling down to room temperature with the furnace.

[0021] The beneficial effects of the present invention are: 1. The present invention prepares an inner glaze that can be used for a ceramic wine bottle. The inner glaze composition includes not only main raw materials such as quartz, feldspar, calcite, and talc, but also metal composite powder as a reinforcing material, and also adds some colorants. The inner glaze prepared by the present invention is not only uniform and smooth on the ceramic wine bottle, but also has strong adhesion and high strength, is not prone to cracks, can well prevent wine leakage, and maintain the freshness and taste of the wine.

[0022] 2. The metal composite powder added to the inner glaze component of the present invention is prepared by using a composite metal salt of iridium and scandium as raw materials, firstly undergoing a complexation treatment with ammonia water, then undergoing a complexation treatment with tricalcium phosphate, and finally undergoing high-temperature sintering. During the preparation process, iridium ions and scandium ions can form an insoluble metal composite complex in ammonia water, and then the composite complex is collected and mixed with tricalcium phosphate by ball milling to form a composite product of tricalcium phosphate / complex, and then undergoing a high-temperature sintering treatment (400-500°C) to form a composite material of metal oxides of iridium and scandium and tricalcium phosphate.

[0023] 3. In the process of forming the inner glaze layer, the glaze needs to undergo a higher temperature baking treatment (850-950°C). During this process, ordinary tricalcium phosphate will slightly decompose and produce bubbles, resulting in an unsmooth glaze surface. However, using the metal composite powder prepared by the present invention to replace the traditional tricalcium phosphate can greatly slow down the generation of bubbles, thereby increasing the density and glossiness of the glaze surface.

[0024] 4. Compared with single iridium or scandium elements, the metal composite powder formed by the composite of iridium and scandium in a certain proportion and tricalcium phosphate in the present invention has better strength and wear resistance and is less prone to cracks, indicating that a benign synergistic coordination is formed between iridium and scandium, which may be related to the formed composite sesquioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0026] Figure 1 This is a product comparison diagram of the inner glaze of the ceramic wine bottle prepared by Example 1 of the present invention and Comparative Example 3. DETAILED DESCRIPTION

[0027] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0028] The present invention will be further described below in conjunction with the following examples. Example 1

[0029] A ceramic wine bottle inner glaze, the ingredients calculated by weight include: 40 parts of quartz stone, 38 parts of potassium feldspar, 24 parts of calcite, 18 parts of talc, 12 parts of metal composite powder, 8 parts of titanium dioxide, 2.4 parts of sodium carboxymethyl cellulose and 35 parts of deionized water.

[0030] The purity of quartz is higher than 99.9%, and the particle size is 10-20μm; the purity of potassium feldspar is higher than 99%, and the particle size is 10-20μm; the purity of calcite is higher than 99.5%, and the particle size is 10-20μm; the purity of talc is higher than 99%, and the particle size is 10-20μm.

[0031] The method for preparing the metal composite powder comprises: S1. Mix iridium trichloride (IrCl3) and scandium trichloride (ScCl3) in deionized water, the mass volume ratio of iridium trichloride, scandium trichloride and deionized water is 0.45g:0.22g:15mL, stir thoroughly until uniform, then drop 25% ammonia water by mass, the amount added is 15% of the volume of deionized water, stir for 8h in an ice water bath, then warm to room temperature, continue stirring for 1.5h, filter out the precipitate, wash with water until the washing liquid is neutral, and obtain a composite complex after vacuum drying; S2, mixing the composite complex and tricalcium phosphate (Ca3(PO4)2) into a ball mill, wherein the mass ratio of the composite complex to tricalcium phosphate is 1:3.5, and ball milling is performed under inert protection, the ball milling speed is 400 r / min, the ball milling time is 5 h, and the ball-to-material ratio is 8:1, to obtain a composite product; S3. The composite product is sintered in a muffle furnace at a sintering temperature of 450° C. for 3 hours to obtain a metal composite powder.

[0032] The method for preparing the inner glaze of the ceramic wine bottle comprises the following steps: The first step is to weigh sodium carboxymethyl cellulose and deionized water according to weight parts, and mix them thoroughly to obtain a dispersion; The second step is to weigh quartz, potassium feldspar, calcite, talc, metal composite powder and titanium dioxide according to weight parts and add them into the dispersion liquid of the first step to obtain a raw material mixed liquid; The third step is to fully mix the raw material mixture in the second step until it is uniform, thereby obtaining the inner glaze slurry; The fourth step is to glaze the inner surface of the ceramic wine bottle body with the inner glaze slurry, and then bake it in a high-temperature furnace, that is, first heat it to 750°C at a rate of 3°C / min, then heat it to 900°C at a rate of 1.5°C / min, keep it warm for 25 minutes, and then cool it to room temperature with the furnace to form the inner glaze of the ceramic wine bottle. Example 2

[0033] A ceramic wine bottle inner glaze, the ingredients calculated by weight include: 30 parts of quartz stone, 25 parts of potassium feldspar, 16 parts of calcite, 12 parts of talc, 8 parts of metal composite powder, 5 parts of magnesium oxide, 1.2 parts of sodium hydroxyethyl cellulose and 30 parts of deionized water.

[0034] The purity of quartz is higher than 99.9%, and the particle size is 10-20μm; the purity of potassium feldspar is higher than 99%, and the particle size is 10-20μm; the purity of calcite is higher than 99.5%, and the particle size is 10-20μm; the purity of talc is higher than 99%, and the particle size is 10-20μm.

[0035] The method for preparing the metal composite powder comprises: S1. Mix iridium trichloride (IrCl3) and scandium trichloride (ScCl3) in deionized water, the mass volume ratio of iridium trichloride, scandium trichloride and deionized water is 0.3g:0.15g:10mL, stir thoroughly until uniform, then drop 20% ammonia water by mass, the amount added is 10% of the volume of deionized water, stir for 5h in an ice water bath, then warm to room temperature, continue stirring for 1h, filter out the precipitate, wash with water until the washing liquid is neutral, and obtain a composite complex after vacuum drying; S2, mixing the composite complex and tricalcium phosphate (Ca3(PO4)2) into a ball mill, wherein the mass ratio of the composite complex to tricalcium phosphate is 1:2.3, and ball milling is performed under inert protection, the ball milling speed is 350 r / min, the ball milling time is 3 h, and the ball-to-material ratio is 6:1, to obtain a composite product; S3. The composite product is sintered in a muffle furnace at a sintering temperature of 400° C. for 2 h to obtain a metal composite powder.

[0036] The method for preparing the inner glaze of the ceramic wine bottle comprises the following steps: The first step is to weigh sodium hydroxyethyl cellulose and deionized water according to weight parts, and mix them thoroughly to obtain a dispersion; The second step is to weigh quartz, potassium feldspar, calcite, talc, metal composite powder and magnesium oxide according to weight parts and add them into the dispersion liquid of the first step to obtain a raw material mixed liquid; The third step is to fully mix the raw material mixture in the second step until it is uniform, thereby obtaining the inner glaze slurry; The fourth step is to glaze the inner surface of the ceramic wine bottle body with the inner glaze slurry, and then bake it in a high-temperature furnace, that is, first heat it to 700°C at a rate of 2°C / min, then heat it to 850°C at a rate of 1°C / min, keep it warm for 20 minutes, and then cool it to room temperature with the furnace to form the inner glaze of the ceramic wine bottle. Example 3

[0037] A ceramic wine bottle inner glaze, the ingredients calculated by weight include: 50 parts of quartz stone, 50 parts of potassium feldspar, 32 parts of calcite, 24 parts of talc, 16 parts of metal composite powder, 10 parts of iron oxide, 3.6 parts of polyacrylamide and 40 parts of deionized water.

[0038] The purity of quartz is higher than 99.9%, and the particle size is 10-20μm; the purity of potassium feldspar is higher than 99%, and the particle size is 10-20μm; the purity of calcite is higher than 99.5%, and the particle size is 10-20μm; the purity of talc is higher than 99%, and the particle size is 10-20μm.

[0039] The method for preparing the metal composite powder comprises: S1. Mix iridium trichloride (IrCl3) and scandium trichloride (ScCl3) in deionized water, the mass volume ratio of iridium trichloride, scandium trichloride and deionized water is 0.6g:0.3g:20mL, stir thoroughly until uniform, then drop 30% ammonia water by mass fraction, the added amount is 20% of the volume of deionized water, stir for 10h in an ice water bath, then warm to room temperature, continue stirring for 2h, filter out the precipitate, wash with water until the washing liquid is neutral, and obtain a composite complex after vacuum drying; S2, mixing the composite complex and tricalcium phosphate (Ca3(PO4)2) into a ball mill, wherein the mass ratio of the composite complex to tricalcium phosphate is 1:4.6, and ball milling is performed under inert protection, the ball milling speed is 450 r / min, the ball milling time is 6 h, and the ball-to-material ratio is 10:1, to obtain a composite product; S3. The composite product is sintered in a muffle furnace at a sintering temperature of 500° C. for 4 hours to obtain a metal composite powder.

[0040] The method for preparing the inner glaze of the ceramic wine bottle comprises the following steps: The first step is to weigh the thickener and deionized water according to the weight ratio, and mix them thoroughly to obtain a dispersion; The second step is to weigh quartz, potassium feldspar, calcite, talc, metal composite powder and colorant according to weight parts and add them into the dispersion liquid of the first step to obtain a raw material mixed liquid; The third step is to fully mix the raw material mixture in the second step until it is uniform, thereby obtaining the inner glaze slurry; The fourth step is to glaze the inner surface of the ceramic wine bottle body with the inner glaze slurry, and then bake it in a high-temperature furnace, that is, first heat it to 800°C at a rate of 4°C / min, then heat it to 950°C at a rate of 2°C / min, keep it warm for 30 minutes, and then cool it to room temperature with the furnace to form the inner glaze of the ceramic wine bottle.

[0041] Comparative Example 1 A ceramic wine bottle inner glaze, which is different from Example 1 only in that the metal composite powder is replaced by tricalcium phosphate (Ca3(PO4)2) powder. The other components and preparation process remain unchanged.

[0042] Calculated by weight, including: 40 parts of quartz stone, 38 parts of potassium feldspar, 24 parts of calcite, 18 parts of talc, 12 parts of tricalcium phosphate (Ca3(PO4)2) powder, 8 parts of titanium dioxide, 2.4 parts of sodium carboxymethyl cellulose and 35 parts of deionized water.

[0043] Comparative Example 2 A ceramic wine bottle inner glaze, which is different from Example 1 only in that the metal composite powder is replaced by iridium / tricalcium phosphate composite powder. The other components and preparation process remain unchanged.

[0044] Calculated by weight, including: 40 parts of quartz stone, 38 parts of potassium feldspar, 24 parts of calcite, 18 parts of talc, 12 parts of iridium / tricalcium phosphate composite powder, 8 parts of titanium dioxide, 2.4 parts of sodium carboxymethyl cellulose and 35 parts of deionized water.

[0045] The preparation method of iridium / tricalcium phosphate composite powder comprises: S1, iridium trichloride was mixed into deionized water, the mass volume ratio of iridium trichloride and deionized water was 0.67g:15mL, and the mixture was stirred until uniform, and then 25% ammonia water was added dropwise, and the amount added was 15% of the volume of deionized water, and the mixture was stirred for 8h under an ice-water bath, and then warmed to room temperature, and stirred for 1.5h, and the precipitate was filtered out, washed with water until the washing solution was neutral, and dried in vacuo to obtain a complex; S2, the complex and tricalcium phosphate are mixed into a ball mill, the mass ratio of the complex and tricalcium phosphate is 1:3.5, and ball milling is performed under inert protection, the ball milling speed is 400r / min, the ball milling time is 5h, and the ball-to-material ratio is 8:1, to obtain a composite product; S3. The composite product is sintered in a muffle furnace at a sintering temperature of 450° C. for 3 h to obtain an iridium / tricalcium phosphate composite powder.

[0046] Comparative Example 3 A ceramic wine bottle inner glaze, which is different from Example 1 only in that the metal composite powder is replaced by iridium / tricalcium phosphate composite powder. The other components and preparation process remain unchanged.

[0047] Calculated by weight, including: 40 parts of quartz stone, 38 parts of potassium feldspar, 24 parts of calcite, 18 parts of talc, 12 parts of iridium / tricalcium phosphate composite powder, 8 parts of titanium dioxide, 2.4 parts of sodium carboxymethyl cellulose and 35 parts of deionized water.

[0048] The preparation method of iridium / tricalcium phosphate composite powder comprises: S1. Mix scandium trichloride with deionized water, the mass volume ratio of scandium trichloride to deionized water is 0.67g:15mL, stir thoroughly until uniform, then add dropwise 25% ammonia water, the amount added is 15% of the volume of deionized water, stir under ice water bath for 8h, then warm to room temperature, continue stirring for 1.5h, filter out the precipitate, wash with water until the washing liquid is neutral, and obtain a complex after vacuum drying; S2, the complex and tricalcium phosphate are mixed into a ball mill, the mass ratio of the complex and tricalcium phosphate is 1:3.5, and ball milling is performed under inert protection, the ball milling speed is 400r / min, the ball milling time is 5h, and the ball-to-material ratio is 8:1, to obtain a composite product; S3. The composite product is sintered in a muffle furnace at a sintering temperature of 450° C. for 3 hours to obtain a scandium / tricalcium phosphate composite powder.

[0049] Experimental example The performance of the ceramic wine bottle inner glaze prepared in Example 1 and Comparative Examples 1-3 was tested and compared, and the test items were: surface state, adhesion, wear resistance and flexural strength. The surface state was obtained by naked eye observation and finger touch; the adhesion test reference standard GB∕T 1720-2020; the wear resistance test reference standard GB / T3810.7-2016; the flexural strength test reference standard GB / T3001-2017.

[0050] The test results are shown in Table 1:

[0051] It can be seen from Table 1 that the inner glaze of the ceramic wine bottle prepared in Example 1 has a smooth and flat surface state, the adhesion can reach level 1, the wear resistance reaches level 5, and the flexural strength is 158MPa, which is better than the performance of Comparative Examples 1-3. It shows that the inner glaze prepared in Example 1 of the present invention is not only uniform and smooth on the ceramic wine bottle, but also has strong adhesion and high strength, is not easy to crack, can well prevent wine leakage, and maintain the freshness and taste of the wine.

[0052] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0053] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A ceramic wine bottle inner glaze, characterized in that: Calculated by weight, including: 30-50 parts of quartz stone, 25-50 parts of potassium feldspar, 16-32 parts of calcite, 12-24 parts of talc, 8-16 parts of metal composite powder, 5-10 parts of colorant, 1.2-3.6 parts of tackifier and 30-40 parts of deionized water.

2. The ceramic wine bottle inner glaze according to claim 1, characterized in that: The purity of the quartz stone is higher than 99.9%, and the particle size is 10-20μm; the purity of the potassium feldspar is higher than 99%, and the particle size is 10-20μm; the purity of the calcite is higher than 99.5%, and the particle size is 10-20μm; the purity of the talc is higher than 99%, and the particle size is 10-20μm.

3. The ceramic wine bottle inner glaze according to claim 1, characterized in that: The colorant is one or a combination of titanium dioxide, magnesium oxide, iron oxide, and calcium borate.

4. The ceramic wine bottle inner glaze according to claim 1, characterized in that: The viscosity enhancer is one or a combination of sodium carboxymethyl cellulose, sodium hydroxyethyl cellulose, polyacrylamide and polyvinyl alcohol.

5. The ceramic wine bottle inner glaze according to claim 1, characterized in that: The preparation method of the metal composite powder comprises: S1. Mix iridium trichloride (IrCl3) and scandium trichloride (ScCl3) in deionized water, stir thoroughly until uniform, then drop ammonia water, stir for 5-10 hours in an ice water bath, then warm to room temperature, continue stirring for 1-2 hours, filter out the precipitate, wash with water until the washing liquid is neutral, and vacuum dry to obtain a composite complex; S2, mixing the composite complex and tricalcium phosphate (Ca3(PO4)2) into a ball mill, and performing ball milling treatment under inert protection to obtain a composite product; S3. Sintering the composite product in a muffle furnace to obtain a metal composite powder.

6. The ceramic wine bottle inner glaze according to claim 5, characterized in that: In S1, the mass volume ratio of iridium trichloride, scandium trichloride and deionized water is (0.3-0.6) g: (0.15-0.3) g: (10-20) mL; the mass fraction of ammonia water is 20%-30%, and the added amount is 10%-20% of the volume of deionized water.

7. The ceramic wine bottle inner glaze according to claim 5, characterized in that: In the S2, the mass ratio of the composite complex to tricalcium phosphate is 1:2.3-4.6; the ball milling speed is 350-450 r / min, the ball milling time is 3-6 h, and the ball-to-material ratio is 6-10:

1.

8. The ceramic wine bottle inner glaze according to claim 5, characterized in that: In S3, the sintering temperature is 400-500° C., and the sintering time is 2-4 hours.

9. A method for preparing the inner glaze of a ceramic wine bottle according to claim 1, characterized in that: The following steps are involved: The first step is to weigh the thickener and deionized water according to the weight ratio, and mix them thoroughly to obtain a dispersion; The second step is to weigh quartz, potassium feldspar, calcite, talc, metal composite powder and colorant according to weight parts and add them into the dispersion liquid of the first step to obtain a raw material mixed liquid; The third step is to fully mix the raw material mixture in the second step until it is uniform, thereby obtaining the inner glaze slurry; The fourth step is to glaze the inner surface of the ceramic wine bottle blank with the inner glaze slurry, and then bake it in a high-temperature furnace to form the inner glaze of the ceramic wine bottle.

10. The method for preparing the inner glaze of a ceramic wine bottle according to claim 9, characterized in that: The calcination process is as follows: firstly, heating to 700-800°C at a rate of 2-4°C / min, then heating to 850-950°C at a rate of 1-2°C / min, keeping the temperature for 20-30 minutes, and then cooling down to room temperature with the furnace.

Citation Information

Patent Citations

  • Jun glaze for wine bottles

    CN109052956A

  • High-capacity high-temperature porcelain wine bottle glaze and preparation method thereof

    CN110903079A

  • Formula and method of ceramic wine bottle vanadium yellow matte decorative glaze

    CN112679091A

  • Sintering method of colored ceramic glaze for wine bottle production

    CN114516763A