NiFe / BiVO4 photo-anode and preparation method and application thereof
By growing NiFe catalyst on the surface of BiVO4, NiFe/BiVO4 composite photoanode is formed, which solves the problem of poor activity and stability of BiVO4 in photoelectro-catalyzed water oxidation, and achieves efficient water oxidation reaction and stability improvement.
Patent Information
- Application Number
- CN202411189372.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
BiVO4 has photogenerated carrier recombination and photogenerated corrosion during photoelectro-catalyzed water oxidation, resulting in poor reaction activity and stability.
The NiFe catalyst is grown on the surface of BiVO4 to form a NiFe/BiVO4 composite photoanode. The preparation method includes pretreatment of FTO glass, electroplating solution preparation, heat treatment and uniform spread of NiFe catalyst to improve the photoelectrocatalytic performance.
The catalytic activity and stability of photoelectro-catalytic water decomposition are improved, and the efficient water oxidation reaction is achieved. The photocurrent density reaches 4.01mA/cm2, and the high stability is maintained at 1.23V vs. RHE.
Smart Images

Figure CN118978344A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoelectrochemistry, and in particular relates to a NiFe / BiVO4 photoanode and a preparation method and application thereof. Background Art
[0002] Since the beginning of the 21st century, the rapid consumption of fossil fuels has caused irreversible damage to the environment. As the most abundant and clean renewable resource on earth, solar energy has always been a hot topic for scientists. Photoelectrocatalytic water splitting technology is an effective method to convert solar energy into hydrogen energy for storage and utilization. How to design a photoanode that can operate efficiently and stably is crucial to the entire water splitting reaction. Among the many semiconductor photoanode materials with photocatalytic activity, BiVO4 has become a widely studied and applied material for photoelectrocatalytic water splitting. However, BiVO4 also has problems such as recombination of photogenerated carriers and serious photogenerated corrosion in the process of photoelectrocatalytic water oxidation, resulting in poor activity and stability of the entire reaction system. Therefore, we modified the BiVO4 surface by growing NiFe catalyst to form a NiFe / BiVO4 composite photoanode, thereby improving its photoelectrocatalytic PEC water splitting performance. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a method for preparing a NiFe / BiVO4 photoanode, comprising the following steps:
[0004] 1) Preparation of BiVO4 photoanode;
[0005] 2) Preparation of NiFe / BiVO4 photoanode: Weigh a certain amount of iron nitrate and nickel nitrate, grind them into powder, evenly spread them on the BiVO4 photoanode, put them into an oven, and when they are molten, take out the photoanode, rinse them with deionized water, and blow dry them with nitrogen to obtain the NiFe / BiVO4 photoanode.
[0006] The above-mentioned NiFe / BiVO4 photoanode, the preparation method of BiVO4 photoanode comprises the following steps:
[0007] 1) Pretreatment of FTO conductive glass: Clean the FTO glass with detergent, acetone, anhydrous ethanol and deionized water in sequence;
[0008] 2) Preparation of electroplating solution: 0.4MKI and 0.04MBi(NO3)3·5H2O were slowly poured into 50mL nitric acid aqueous solution in sequence, and stirred vigorously until completely dissolved. The solution gradually turned orange-red. 0.23M p-benzoquinone was prepared and dissolved in 20mL anhydrous ethanol by ultrasonic dissolution. Then it was mixed with the orange-red solution. After mixing, the solution turned dark red.
[0009] 3) Immerse FTO in the prepared electroplating solution with a size of 1cm×1cm as the working electrode, use Pt wire as the counter electrode, and use Ag / AgCl as the reference electrode; use a three-electrode system with an input voltage of -0.1Vvs.Ag / AgCl, electroplate for 300 seconds, and make a BiOI glass plate with uniform thickness;
[0010] 4) Prepare 0.4M vanadyl acetylacetonate and dissolve it in 1.0mL DMSO. Mix well and take 20.0μL to drop on the surface of BiOI glass plate. Place the drop-coated BiOI glass plate in a muffle furnace and heat for 2 hours.
[0011] 5) Prepare 1M NaOH solution to remove V2O5 on the surface of BiVO4. After the surface of the BiVO4 plate turns golden yellow, rinse it with deionized water and blow dry it with N2 to obtain a BiVO4 photoanode.
[0012] In the above-mentioned NiFe / BiVO4 photoanode, in step 4), the temperature in the muffle furnace is increased to 450°C at a heating rate of 2°C / min.
[0013] In the above-mentioned NiFe / BiVO4 photoanode, in step 2), the pH of the nitric acid aqueous solution is 1.7.
[0014] In the above-mentioned NiFe / BiVO4 photoanode, in step 2), the iron nitrate and nickel nitrate are weighed in a mass ratio of 2:1.
[0015] The electrochemical performance test method is as follows:
[0016] 1) An electrochemical workstation CHI660 was used, with NiFe / BiVO4 photoanode as the working electrode, Pt wire as the counter electrode, Ag / AgCl as the reference electrode, and the electrolyte being potassium borate solution with a pH of 9.3.
[0017] 2) The scan rate of linear sweep voltammetry is 0.05 Vs -1 .
[0018] The beneficial effect of the present invention is that the present invention adopts a simple and rapid preparation method to grow a layer of NiFe catalyst on the BiVO4 photoanode to obtain a NiFe / BiVO4 photoanode. At 1.23V vs. RHE, the photocurrent density reaches 4.01mA / cm 2 . The catalytic activity of photoelectrocatalytic water splitting was improved to a certain extent, while the photoelectrocatalytic stability was also enhanced, achieving efficient water oxidation reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a transmission electron microscope image of the BiVO4 photoanode.
[0020] Figure 2 This is a transmission electron microscope image of the NiFe / BiVO4 photoanode.
[0021] Figure 3 are the X-ray diffraction patterns (XRD) of BiVO4 photoanode and NiFe / BiVO4 photoanode.
[0022] Figure 4 These are the linear sweep voltammetry curves of BiVO4 photoanode and NiFe / BiVO4 photoanode.
[0023] Figure 5 Chronoamperometric curves (it) of BiVO4 and NiFe / BiVO4 photoanodes at 0.8 V vs. RHE. DETAILED DESCRIPTION
[0024] Example 1 Preparation of NiFe / BiVO4 Photoanode
[0025] Pretreatment of FTO conductive glass: put the FTO glass into a solution containing detergent for ultrasonic cleaning for 30 minutes, rinse it with deionized water, then put it into an acetone solution for ultrasonic cleaning for 30 minutes, and finally put it into an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, blow dry it with nitrogen and set it aside;
[0026] Preparation of electroplating solution: Prepare 50mL of 0.4MKI and 0.04MBi(NO3)3·5H2O solution, slowly pour them into a nitric acid aqueous solution with a pH of 1.7, stir vigorously until completely dissolved, and the solution gradually turns orange-red. Prepare 20mL of 0.23M p-benzoquinone and dissolve it in anhydrous ethanol by ultrasonic dissolution, then mix it with the orange-red solution, and the solution turns dark red after mixing;
[0027] Preparation of BiVO4 photoanode: After the above electroplating solution is prepared, immerse FTO in the prepared electroplating solution with a size of 1cm×1cm as the working electrode, Pt wire as the counter electrode, and Ag / AgCl as the reference electrode; use a three-electrode system with an input voltage of -0.1Vvs.Ag / AgCl, electroplating for 300 seconds to make a BiOI glass plate with uniform thickness. Then prepare 1mL of 0.4M acetylacetonatovanadium oxydissolved in DMSO, mix well and take 20.0μL to drop on the surface of the BiOI glass plate, place the drop-coated BiOI glass plate in a muffle furnace and heat it to 450℃ at a heating rate of 2℃ / min, and continue heating for 2 hours. After the heating program is completed, prepare 1MNaOH solution to remove V2O5 on the surface of BiVO4. After the surface of the BiVO4 plate turns golden yellow, rinse it with deionized water, blow dry it with N2, and obtain the BiVO4 photoanode.
[0028] Preparation of NiFe / BiVO4 photoanode: Weigh a certain amount of iron nitrate and nickel nitrate, grind them into powder according to the mass ratio of 2:1, evenly spread them on the BiVO4 photoanode, put them into an oven, and when they are in a molten state, take out the photoanode, rinse it with deionized water, and blow dry it with nitrogen to obtain a NiFe / BiVO4 photoanode.
[0029] Example 2 Electrochemical Performance Test
[0030] Electrochemical performance test: This experiment uses Shanghai Chenhua electrochemical workstation CHI660E, three-electrode system for electrochemical performance research, NiFe / BiVO4 composite photoanode as working electrode, Pt wire as counter electrode, Ag / AgCl as reference electrode, and electrolyte is potassium borate solution with pH=9.3. During the experiment, the xenon light intensity was measured to be 100mW / cm 2 The scanning rate is 50mV·s -1 According to the Nernst equation, E RHE =E Ag / AgCl +0.0591×pH+0.197V. During the experiment, all potentials measured by the reference Ag / AgCl electrodes need to be converted into potentials relative to the reversible hydrogen electrode (RHE).
[0031] Figure 1 This is a transmission electron microscope image of the BiVO4 photoanode. It can be seen that the worm-like structure is 200nm and is evenly distributed, proving that the BiVO4 photoanode was successfully prepared.
[0032] Figure 2 This is a transmission electron microscope image of the NiFe / BiVO4 composite photoanode. Figure 1 It can be seen that there is a layered catalyst attached to the surface of the BiVO4 photoanode, proving that the NiFe / BiVO4 composite photoanode was successfully prepared.
[0033] Figure 3 The X-ray diffraction patterns of BiVO4 photoanode and NiFe / BiVO4 photoanode. Figure 3 It can be found that loading other catalysts on the surface of bismuth vanadate does not change the structure of bismuth vanadate.
[0034] Figure 4 The linear sweep voltammetry curves of BiVO4 photoanode and NiFe / BiVO4 photoanode are shown in Figure 2. Figure 4 By comparison, it can be found that the unmodified BiVO4 photoanode has the lowest photocurrent density, which is 1.74 mA / cm 2 The photocurrent density of the NiFe / BiVO4 composite photoanode was significantly increased to 4.01 mA / cm 2, the photocurrent density was improved by the modification of NiFe catalyst, and efficient water oxidation reaction was achieved. The increase in photocurrent density may be due to the fact that the introduction of NiFe catalyst increased the conductivity of the photoanode and promoted electron transfer, thereby improving the water oxidation performance.
[0035] Figure 5 The chronoamperometric curves of BiVO4 and NiFe / BiVO4 photoanodes at 0.8 V vs. RHE are shown in Figure 2. By comparison, the stability of the photocurrent density of the NiFe / BiVO4 composite photoanode remains at 99% within 3600 s, which may be due to the combination of the NiFe catalyst making the structure of the composite photoanode more stable, thereby improving the stability of the photoelectrode.
Claims
1. A NiFe / BiVO4 photoanode, characterized in that: The preparation method comprises the following steps: 1) Preparation of BiVO4 photoanode; 2) Preparation of NiFe / BiVO4 photoanode: Weigh a certain amount of iron nitrate and nickel nitrate, grind them into powder, evenly spread them on the BiVO4 photoanode, put them into an oven and heat them. When they are in a molten state, take out the photoanode, rinse them with deionized water, and blow dry them with nitrogen to obtain a NiFe / BiVO4 photoanode.
2. A NiFe / BiVO4 photoanode according to claim 1, characterized in that: The preparation method of BiVO4 photoanode comprises the following steps: 1) Pretreatment of FTO conductive glass: Clean the FTO glass with detergent, acetone, anhydrous ethanol and deionized water in sequence; 2) Preparation of electroplating solution: 0.4M KI and 0.04MBi(NO3)3·5H2O were slowly poured into 50mL nitric acid aqueous solution in sequence, and stirred vigorously until completely dissolved. The solution gradually turned orange-red. 0.23M p-benzoquinone was prepared and dissolved in 20mL anhydrous ethanol by ultrasonic dissolution. Then it was mixed with the orange-red solution. After mixing, the solution turned dark red. 3) Immerse FTO in the prepared electroplating solution with a size of 1cm×1cm as the working electrode, use Pt wire as the counter electrode, and use Ag / AgCl as the reference electrode; use a three-electrode system with an input voltage of -0.1Vvs.Ag / AgCl, electroplate for 300 seconds, and make a BiOI glass plate with uniform thickness; 4) Prepare 0.4M vanadium acetylacetonate and dissolve it in 1.0mL DMSO. Mix well and take 20.0μL of it and drop it on the surface of BiOI glass plate. Place the drop-coated BiOI glass plate in a muffle furnace and heat it. 5) Prepare 1M NaOH solution to remove V2O5 on the surface of BiVO4. After the surface of the BiVO4 plate turns golden yellow, rinse it with deionized water and blow dry it with N2 to obtain a BiVO4 photoanode.
3. A NiFe / BiVO4 photoanode according to claim 2, characterized in that: In step 4), the heating in the muffle furnace is to increase the temperature to 450° C. at a heating rate of 2° C. / min for 2 hours.
4. A NiFe / BiVO4 photoanode according to claim 2, characterized in that: In step 2), the pH of the nitric acid aqueous solution is 1.
7.
5. The NiFe / BiVO4 photoanode according to claim 1, characterized in that: In step 2), the ferric nitrate and nickel nitrate are weighed in a mass ratio of 2:
1.
6. Use of a NiFe / BiVO4 photoanode as claimed in claim 1 in photoelectrocatalytic water decomposition.
Citation Information
Patent Citations
FeOOH / In-BiVO4 (L) photoelectric anode material as well as preparation method and application thereof
CN115611373A
NiFe / CdS / bismuth vanadate composite photoelectrocatalysis anode material and preparation and application thereof
CN115747828A
Synthesis of high-surface-area nanoporous bivo4 electrodes
US20150361566A1
Cited By
Preparation method and application of BiVO4 / CuFe2O4 composite photo-anode
CN119913559A