Electron blocking material with thick polycyclic structure and organic electroluminescent device thereof

By using electron barrier materials with dense multi-ring structure in organic electroluminescent devices, the problem of insufficient thermal stability and hole transport characteristics of the material in the prior art is solved, and the device life and efficiency are improved. for high-performance organic electroluminescent devices.

CN118978533APending Publication Date: 2024-11-19JILIN YUANHE ELECTRONICS MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411035677.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The thermal stability and hole transport characteristics of electron barrier materials in existing organic electroluminescent devices are insufficient, resulting in a short device life and a high driving voltage, making it difficult to meet application needs.

Method used

Using electron barrier materials with a dense polycyclic structure, the electron-rich adamantane structure is screwed to improve the overall structural immobilization stability of the molecule, and the energy band gap is adjusted through substituents to improve the interface properties and improve the Hole mobility and thermal stability.

Benefits of technology

It improves the life and efficiency of organic electroluminescent devices, reduces the driving voltage, and enhances the film phase stability, avoids crystallization, and expands the use of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978533A_ABST
    Figure CN118978533A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of organic electroluminescent materials, and particularly relates to an electron blocking material with a thick polycyclic structure and an organic electroluminescent device thereof. According to the present invention, the adamantane structure contains the electron-rich adamantane structure and the fused polycyclic structure screwed with the adamantane, the adamantane structure with the large molecular weight has rigidity, and after the adamantane structure with the large molecular weight is screwed with the rigid fused polycyclic structure, the overall structure immobilization stability of the molecule is improved so as to prolong the service life of the device; compared with a hole transport material of a contrast compound, the compound provided by the invention has a relatively deep HOMO energy level, so that an injection barrier between the hole transport material and a main body material is smaller, the driving voltage of a device is reduced, and the efficiency of the device is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic electroluminescent materials, and in particular relates to an electron blocking material with a condensed polycyclic structure and an organic electroluminescent device thereof. Background Art

[0002] In the field of small and medium-sized panels, the shipment volume of organic electroluminescent devices (OLEDs) has surpassed that of liquid crystal displays (LCDs) in 2024. As the application scenarios of OLEDs become more and more diverse, the requirements for the performance of organic electroluminescent materials are also becoming higher and higher. Obtaining high-efficiency and long-life devices remains the most important goal for their commercialization.

[0003] The materials used in OLEDs include carrier injection materials (hole injection materials, electron injection materials), carrier transport materials (hole transport materials, electron transport materials), luminescent materials (luminescent host materials, luminescent guest materials), etc. according to their functions. According to the order of evaporation materials used to prepare devices, hole transport materials are divided into hole transport materials and electron blocking materials. The main function of the first layer of hole transport materials is to transport holes, and the second layer of electron blocking materials has the function of confining electrons, so that excitons are generated in the luminescent layer without electrons escaping. Therefore, the electron blocking material is not only required to have a high Tg and thermal stability, but also to have good hole transport properties and a suitable highest occupied orbital (HOMO). Summary of the invention

[0004] In order to solve the problems existing in the background technology, the first object of the present invention is to provide an electron blocking material having a condensed polycyclic structure, and the technical solution is as follows:

[0005] An electron blocking material having a condensed polycyclic structure has a structure shown in the following general formula I:

[0006]

[0007] Wherein X is selected from a single bond, CR 1 R 2 , O, S or S(=O)2; Y is selected from CR 3 R 4 , O, S; Z1 is selected from a single bond, CR 5 R 6 , O, S or S(=O)2; Z2 is selected from a single bond, CR 7 R 8 , O, S or S(=O)2;

[0008] R 1 To R 8 are the same or different from each other and are independently selected from hydrogen, C1 to C 10 Alkyl, C6~C 30The aryl group; R 9 To R 12 are the same or different from each other and are independently selected from deuterium, cyano, amine, halogen, C1-C 10 Alkyl, C6~C 30 The aryl group, n is independently selected from 0 to the maximum number of sites that can be substituted in the ring.

[0009] As a preferred embodiment of the present invention, X is selected from a single bond, CR 1 R 2 , O, S; Z1 is selected from a single bond, CR 5 R 6 , O, S; Z2 is selected from a single bond, CR 7 R 8 , O, S.

[0010] As a preferred embodiment of the present invention, when X is a single bond, Z1 is a single bond, Z2 is a single bond; X is CR 1 R 2 When Z1 is CR 5 R 6 , Z2 is CR 7 R 8 ; When X is O, Z1 and Z2 are O; When X is S, Z1 and Z2 are S; General Formula I is represented by the following formulas (1-1) to (1-4):

[0011]

[0012] As a preferred embodiment of the present invention, the R 1 , R 2 The same as each other, selected from methyl or phenyl: the R 3 , R 4 are the same as each other and are methyl; the R 5 , R 6 are the same as each other and are selected from methyl or phenyl; said R 7 , R 8 are the same as each other and are selected from methyl or phenyl; n is 0.

[0013] As a preferred embodiment of the present invention, the structure of the general formula I is as follows:

[0014]

[0015]

[0016]

[0017]

[0018]

[0019]

[0020] Another object of the present invention is to provide an organic electroluminescent device, comprising a first electrode, a second electrode and an organic material layer arranged therebetween, wherein the organic material layer comprises a hole transport material, and the hole transport material comprises at least one of the above-mentioned electron blocking materials having a condensed polycyclic structure.

[0021] As a preferred embodiment of the present invention, the organic electroluminescent device is applied to a flat panel display device or a flexible display device.

[0022] The beneficial effects of the present invention are as follows:

[0023] The electronic blocking material with thick polycyclic structure provided by the present invention comprises an electron-rich adamantane structure, a thick polycyclic structure connected with adamantane, wherein the adamantane structure of high molecular weight has rigidity, and after being connected with the rigid thick polycyclic structure, the overall structure immobilization stability of the molecule is improved, thereby improving the device life, and adamantane itself is a three-dimensional molecular structure, which can regulate the thermal stability of the compound, and can effectively prevent the aggregation between molecules, and the film phase stability is strong, so that the compound is not easy to crystallize. The thick polycyclic structure containing ten rings has a strong planarity, which is conducive to improving the mobility of holes. And the compound provided by the present invention has a relatively deep HOMO energy level compared to the hole transport material of the comparison compound, so that the injection barrier between the hole transport material and the host material is smaller, which is conducive to reducing the driving voltage of the device, and effectively improving the device efficiency, thereby improving the life of the device.

[0024] In addition, by introducing various substituents into the core structure, the energy band gap can be fine-tuned while improving the interfacial properties between organic materials, diversifying the uses of the materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0026] Figure 1 is the DSC spectrum of the prepared compound 1;

[0027] Figure 2 The chem3D geometry optimization diagram of the prepared compound 1;

[0028] Figure 3 Graph showing the lifetime of the organic electroluminescent device in device example 1 and device comparison example 1. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] If the specific conditions are not specified in the embodiments, they are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. Some reaction compounds are purchased from commodity suppliers (Zhengzhou Alpha Chemical Co., Ltd.), and some compounds that cannot be directly purchased are prepared by simple reactions of commercially available raw materials. The percentages all refer to mass percentages, and the temperatures are degrees Celsius (℃). Such method principles, operating procedures, conventional post-treatments, silica gel columns, recrystallization purification and other means are well known to synthesizers in the art, and the synthesis process can be fully realized to obtain the target product. The reactions in each preparation embodiment are generally carried out under positive pressure of nitrogen or argon.

[0031] Preparation Example

[0032] Example 1: Preparation of Compound 1

[0033]

[0034] Synthesis of compound 1-3: Compound 1-1 (8.6 g, 16 mmol), compound 1-2 (5.8 g, 16 mmol), palladium acetate (0.2 g, 1 mmol), sodium tert-butoxide (3.1 g, 32 mmol), bis(diphenylphosphino)-1,1'-binaphthyl (0.6 g, 1 mmol) and toluene (45 mL) were placed in a 100 mL reactor. The mixture was refluxed for 2 hours under stirring. After the reaction was completed, the filtrate was concentrated and purified by column chromatography to obtain compound 1-3 (10.0 g, yield 81%);

[0035] Synthesis of compound 1: Compound 1-3 (19.4 g, 25 mmol), Pd(OAc)2 (0.44 g, 2 mmol), PCy3HBF4 (1.48 g, 4 mmol) and K2CO3 (0.82 g, 6 mmol) were dispersed in DMAc and reacted at 130°C for 24 h. After cooling to room temperature, the filter cake was filtered under reduced pressure, and the crude product was purified by silica gel column chromatography (DCM as eluent) to obtain compound 1 (11.5 g, yield 75%), MS: 615.42.

[0036] Example 2: Preparation of Compound 5

[0037]

[0038] Synthesis of compound 5-3: The synthesis method is the same as that of compound 1-3, except that compound 1-1 is replaced by compound 5-1, and compound 1-2 is replaced by compound 5-2;

[0039] Synthesis of compound 5: n-BuLi (1.40 g, 22 mmol) was slowly dripped into a dry t-BuPh solution of compound 5-3 (7.9 g, 10 mmol) under N2 atmosphere, reacted at 0°C for 2 h, acetone (1.28 g, 22 mmol) t-BuPh solution was slowly dripped, and then naturally warmed to room temperature. The reaction was quenched with H2O, the organic layer solvent was removed by rotary evaporation, the crude product was purified by Al2O3 column chromatography (ethyl acetate / petroleum ether, volume ratio 1:10), and recrystallized from THF and MeOH to obtain an intermediate; HCl was slowly dripped into a CH3COOH solution of the intermediate and stirred for 10 min, and the filter cake was quickly vacuum filtered, washed with MeOH, and then recrystallized from THF and MeOH to obtain compound 5 (5.9 g, yield 83%), MS: 715.50.

[0040] Example 3: Preparation of Compound 9

[0041]

[0042] Synthesis of compound 9-3: The synthesis method is the same as that of compound 1-3, except that compound 1-1 is replaced by compound 9-1, and compound 1-2 is replaced by compound 9-2;

[0043] Synthesis of compound 9: Compound 9-3 (40.8 g, 50 mmol), potassium carbonate (27.6 g, 200 mmol) and N-methyl-2-pyrrolidone (1.6 L) were added to a 2 L three-necked flask and stirred at 150 ° C for 12 hours. After the reaction was completed, the reaction product was separated, the organic layer was concentrated under reduced pressure, separated by column chromatography, and dried to obtain compound 9 (25.5 g, yield 78%), MS: 653.34.

[0044] Example 4: Preparation of Compound 11

[0045]

[0046] Synthesis of compound 11-3: The synthesis method is the same as that of compound 1-3, except that compound 11-1 is used to replace compound 1-1, and compound 11-2 is used to replace compound 1-2;

[0047] Synthesis of compound 11-4: Under N2 atmosphere, LaCl3·2LiCl (7.2g, 22mmol) in THF was kept at -50℃ for 15min, and then n-BuLi (1.4g, 22mmol) was added dropwise, and the mixture was reacted at -50℃ for 30min to obtain n-Bu2LaCl·4LiCl solution. Compound 11-3 (7.8g, 10mmol) in THF (10mL) was added dropwise to n-Bu2LaCl·4LiCl solution, kept at -50℃ for 5min, and reacted at 0℃ for 30min. I2 (50.68g, 200mmol) was added and reacted at room temperature for 1h. The reaction was quenched with water, washed three times with DCM, and the organic solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (DCM / petroleum ether, volume ratio 1:5), and recrystallized with DCM and methanol to obtain compound 11-4 (9.0g, yield 80%).

[0048] Synthesis of compound 11: Under N2 atmosphere, compound 11-4 (11.3 g, 10 mmol), sulfur powder (1.28 g, 40 mmol), KOH (4.48 g, 80 mmol) were dispersed in DMSO and reacted at 110°C for 24 h. The reaction was quenched with water, washed three times with DCM, and the organic solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (DCM / petroleum ether, volume ratio 1:10), and recrystallized with DCM and methanol to obtain compound 11 (5.1 g, yield 75%), MS: 685.28.

[0049] Example 5: Preparation of Compound 61

[0050]

[0051] Synthesis of compound 61-3: The synthesis method is the same as that of compound 1-3, except that compound 1-1 is replaced by compound 61-1, and compound 1-2 is replaced by compound 61-2;

[0052] Synthesis of compound 61-4: Compound 61-3 (19.4 g, 25 mmol), Pd(OAc)2 (0.22 g, 1 mmol), PCy3HBF4 (0.74 g, 2 mmol) and K2CO3 (0.41 g, 3 mmol) were dispersed in DMAc and reacted at 130°C for 24 h. After cooling to room temperature, the filter cake was obtained by filtration under reduced pressure. The crude product was purified by silica gel column chromatography (DCM as eluent) to obtain compound 61-4 (14.2 g, yield 82%);

[0053] Synthesis of compound 61: n-BuLi (0.70 g, 11 mmol) was slowly dripped into a dry t-BuPh solution of compound 61-3 (7.8 g, 10 mmol) under N2 atmosphere, reacted at 0°C for 2 h, acetone (0.64 g, 11 mmol) t-BuPh solution was slowly dripped, and then naturally warmed to room temperature. The reaction was quenched with H2O, the organic layer solvent was removed by rotary evaporation, the crude product was purified by Al2O3 column chromatography (ethyl acetate / petroleum ether, volume ratio 1:10), and recrystallized from THF and MeOH to obtain an intermediate; HCl was slowly dripped into a CH3COOH solution of the intermediate and stirred for 10 min, and the filter cake was quickly vacuum filtered, washed with MeOH, and then recrystallized from THF and MeOH to obtain compound 61 (5.1 g, yield 78%), MS: 657.47.

[0054] Example 6: Preparation of Compound 72

[0055]

[0056] Synthesis of compound 72-3: The synthesis method is the same as that of compound 1-3, except that compound 1-1 is replaced by compound 72-1, and compound 1-2 is replaced by compound 72-2;

[0057] Synthesis of compound 72-4: Under N2 atmosphere, LaCl3·2LiCl (3.6 g, 11 mmol) in THF was kept at -50°C for 15 min, and n-BuLi (0.70 g, 11 mmol) was added dropwise, and the reaction was carried out at -50°C for 30 min to obtain n-Bu2LaCl·4LiCl solution. Compound 72-3 (8.2 g, 10 mmol) in THF (10 mL) was added dropwise to n-Bu2LaCl·4LiCl solution, kept at -50°C for 5 min, and reacted at 0°C for 30 min. I2 (25.38 g, 100 mmol) was added, and the reaction was carried out at room temperature for 1 h. The reaction was quenched with water, washed three times with DCM, and the organic solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (DCM / petroleum ether, volume ratio 1:5), and recrystallized with DCM and methanol to obtain compound 72-4 (7.5 g, yield 76%);

[0058] Synthesis of compound 72-5: Under N2 atmosphere, compound 72-4 (9.9 g, 10 mmol), sulfur powder (0.64 g, 20 mmol), KOH (2.24 g, 40 mmol) were dispersed in DMSO and reacted at 110°C for 24 h. The reaction was quenched with water, washed three times with DCM, and the organic solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (DCM / petroleum ether, volume ratio 1:10), and recrystallized with DCM and methanol to obtain compound 72-5 (5.6 g, yield 73%).

[0059] Synthesis of compound 72: Compound 72-5 (38.3 g, 50 mmol), potassium carbonate (13.8 g, 100 mmol) and N-methyl-2-pyrrolidone (800 mL) were added to a 2L three-necked flask and stirred at 150°C for 12 hours. After the reaction, the reaction product was separated, the organic layer was concentrated under reduced pressure, separated by column chromatography, and dried to obtain compound 72 (23.9 g, yield 70%), MS: 685.28.

[0060] Example 7: Preparation of Compound 85

[0061]

[0062] Synthesis of compound 85-3: The synthesis method is the same as that of compound 1-3, except that compound 1-1 is replaced by compound 85-1, and compound 1-2 is replaced by compound 85-2;

[0063] Synthesis of compound 85-4: Compound 85-3 (20.5 g, 25 mmol), Pd(OAc)2 (0.22 g, 1 mmol), PCy3HBF4 (0.74 g, 2 mmol) and K2CO3 (0.41 g, 3 mmol) were dispersed in DMAc and reacted at 130°C for 24 h. After cooling to room temperature, the filter cake was obtained by filtration under reduced pressure. The crude product was purified by silica gel column chromatography (DCM as eluent) to obtain compound 85-4 (14.0 g, yield 76%);

[0064] Synthesis of compound 85: n-BuLi (0.70 g, 11 mmol) was slowly dripped into a dry t-BuPh solution of compound 85-3 (8.2 g, 10 mmol) under N2 atmosphere, reacted at 0°C for 2 h, acetone (0.64 g, 11 mmol) t-BuPh solution was slowly dripped, and then naturally warmed to room temperature. The reaction was quenched with H2O, the organic layer solvent was removed by rotary evaporation, the crude product was purified by Al2O3 column chromatography (ethyl acetate / petroleum ether, volume ratio 1:10), and recrystallized from THF and MeOH to obtain an intermediate; HCl was slowly dripped into a CH3COOH solution of the intermediate and stirred for 10 min, and the filter cake was quickly vacuum filtered, washed with MeOH, and then recrystallized from THF and MeOH to obtain compound 85 (5.7 g, yield 81%), MS: 699.52.

[0065] In addition, it should be noted that other compounds of the present application can be obtained by referring to the preparation methods of the above-listed embodiments and existing synthesis methods, so they will not be listed one by one here.

[0066] Device Embodiment

[0067] Preparation of organic electroluminescent devices:

[0068] A glass substrate coated with ITO (indium tin oxide) as a thin film with a thickness of 1000 angstroms was placed in distilled water in which a detergent was dissolved and ultrasonically cleaned. After the ITO was cleaned for 30 minutes, ultrasonic cleaning was repeated twice with distilled water for 10 minutes, and then the substrate was ultrasonically cleaned with isopropyl alcohol, acetone and methanol solvents, dried, transferred to a plasma cleaner for cleaning for 5 minutes, and then transferred to a vacuum depositor;

[0069] On the ITO transparent electrode, the compound [HI] was thermally vacuum deposited to a thickness of 100 angstroms to form a hole injection layer; the compound [HT] was vacuum deposited to 800 angstroms on the hole injection layer to form a hole transport layer; the compound 1 was vacuum deposited to a thickness of 50 angstroms on the hole transport layer to form an electron blocking layer (also called a light-emitting auxiliary layer); the compound [BH] and the compound [BD] were vacuum deposited to a thickness of 200 angstroms at a ratio of 97:3 on the electron blocking layer to form a light-emitting layer; the compound [ET] and the compound [LiQ] (lithium quinoline) were vacuum deposited at a ratio of 1:1 to form an electron transport layer with a thickness of 300 angstroms; yttrium (Yb) and magnesium silver (1:9) were sequentially deposited on the electron transport layer to a thickness of 10 angstroms and 1000 angstroms, respectively, to form a cathode. The vacuum degree during deposition was maintained at 1×10 -7 Up to 5×10 -8 Entrust.

[0070] Preparation of device examples 2-7:

[0071] When forming the electron blocking layer, the compound shown in Table 1 was used instead of the compound 1 in Example 1, and an organic electroluminescent device was prepared by the same method as Example 1.

[0072] Preparation of Comparative Examples 1 and 2:

[0073] An organic electroluminescent device was prepared in the same manner as in Example 1, except that Comparative Compound 1 and Comparative Compound 2 were used instead of Compound 1 in Example 1 when forming the electron blocking layer.

[0074] The structure of the compound used in the above preparation process is as follows:

[0075]

[0076]

[0077] The HOMO value of each compound was calculated by Gaussian calculation software; for the organic electroluminescent devices manufactured using each compound as an electron blocking layer in the embodiments and comparative examples, the ... 2 The driving voltage and current efficiency were measured at a current density of 50 mA / cm 2 The time required for the brightness to decrease to 97% of the initial brightness (LT97) was measured at a current density of 1.5 Å. The results are shown in Table 1 below:

[0078] Table 1

[0079]

[0080] In Table 1 above, compared with the comparative example, at the same current density, it can be seen that the current efficiency of the device embodiment is improved, the driving voltage is reduced, and the service life is improved. For example Figure 3 The lifespan comparison diagram of the devices prepared in Comparative Example 1 and Example 1, J = 50 mA / cm 2 At this current density, the brightness drops to 970cd / m 2 The life of the device prepared in Example 1 is longer than that of the device prepared in Comparative Example 1. Figure 2 It can be seen that the molecular structure of the adjusted compound 1 is very planar and its glass transition temperature is high (see Figure 1 , Tg value 144.96°C), so the film forming stability is good during the thermal evaporation process, which is beneficial to improving the life of the device. Moreover, compared with the comparative example compounds, the compounds provided in the present application have a deeper HOMO energy level and can better form ohmic contact with the main material, which is beneficial to reducing the driving voltage of the device and effectively improving the device efficiency, thereby improving the life of the device and having broad application prospects.

Claims

1. An electron blocking material having a condensed polycyclic structure, characterized in that: It has the structure shown in the following general formula I: Wherein X is selected from a single bond, CR 1 R 2 , O, S or S(=O)2; Y is selected from CR 3 R 4 , O, S; Z1 is selected from a single bond, CR 5 R 6 , O, S or S(=O)2; Z2 is selected from a single bond, CR 7 R 8 , O, S or S(=O)2; R 1 To R 8 are the same or different from each other and are independently selected from hydrogen, C1 to C 10 Alkyl, C6~C 30 The aryl group; R 9 To R 12 are the same or different from each other and are independently selected from deuterium, cyano, amine, halogen, C1-C 10 Alkyl, C6~C 30 The aryl group, n is independently selected from 0 to the maximum number of sites that can be substituted in the ring.

2. The electron blocking material having a condensed polycyclic structure according to claim 1, characterized in that: The X is selected from a single bond, CR 1 R 2 , O, S; Z1 is selected from a single bond, CR 5 R 6 , O, S; Z2 is selected from a single bond, CR 7 R 8 , O, S.

3. The electron blocking material having a condensed polycyclic structure according to claim 2, characterized in that: When X is a single bond, Z1 is a single bond, Z2 is a single bond; X is CR 1 R 2 When Z1 is CR 5 R 6 , Z2 is CR 7 R 8 ; When X is O, Z1 and Z2 are O; When X is S, Z1 and Z2 are S; General Formula I is represented by the following formulas (1-1) to (1-4):

4. The electron blocking material having a condensed polycyclic structure according to claim 3, characterized in that: The R 1 , R 2 The same as each other, selected from methyl or phenyl: the R 3 , R 4 are the same as each other and are methyl; 5 , R 6 are the same as each other and are selected from methyl or phenyl; said R 7 , R 8 are the same as each other and are selected from methyl or phenyl; n is 0.

5. The electron blocking material having a condensed polycyclic structure according to claim 1, characterized in that: The structure of the general formula I is as follows:

6. An organic electroluminescent device, characterized in that: It comprises a first electrode, a second electrode and an organic material layer arranged therebetween, wherein the organic material layer comprises a carrier blocking layer, and the preparation material of the carrier blocking layer comprises at least one electron blocking material having a condensed polycyclic structure as described in any one of claims 1-5.

7. The organic electroluminescent device according to claim 6, characterized in that: The organic electroluminescent device is applied to a flat panel display device or a flexible display device.