High-elasticity foaming polyurethane coiled material and preparation method thereof
Through the combination of raw materials such as high fluorine-containing polyols and silicified chain extenders, combined with modified hollow glass microbeads and antioxidants, the problem of polyurethane coils being prone to aging and degraded performance outside is solved, and high elasticity and impact resistance are achieved , waterproof and yellowing resistance.
Patent Information
- Application Number
- CN202411094001.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyurethane coils are easy to absorb rainwater when used outdoors, resulting in accelerated aging and yellowing. The polarity difference between the filled hollow glass microbeads and polymers is large, resulting in reduced material performance and insufficient temperature and impact resistance. .
Using high fluorine-containing polyols, silicified chain extenders, modified hollow glass microbeads, plasticizers, antioxidants and 3-perfluorohexylpropanol, etc., the high-quality materials are prepared through specific ratios and processes. Elastic foamed polyurethane coil, the modified hollow glass microbeads and polyurethane elastomers are grafted through chemical bonds to improve physical compatibility, and improve waterproofing and light resistance through high content of C-F bonds and fluorocarbon groups.
It significantly improves the impact, heat insulation, waterproof and yellowing resistance of the coil material, enhances the mechanical properties and high temperature resistance, delays the aging process, and improves the overall performance of the material.
Smart Images

Figure BDA0004987344220000121 
Figure BDA0004987344220000131
Abstract
Description
[Technical field]
[0001] The invention relates to the technical field of cross-linked polymer foam coiled materials, and in particular to a high-elasticity foamed polyurethane coiled material and a preparation method thereof. [Background technology]
[0002] Foamed polyurethane elastomers are widely used in various industrial fields, such as rubber rollers, sealing gaskets, shoe soles, solid tires, tapes, mechanical parts, caulking materials, paving materials, etc. Due to the high elasticity and wear resistance of polyurethane elastomers, they are increasingly used in paving various sports venues such as plastic tracks in athletic fields, plastic tennis courts, plastic basketball courts and plastic badminton courts.
[0003] Polyurethane foam coils are prepared by reaction foaming. However, foam coil products have problems such as high density, poor temperature resistance, and easy cracking. Usually, inorganic fillers are added during preparation. Among inorganic fillers, rigid hollow microspheres such as hollow glass microspheres and hollow ceramic microspheres contain inert gases, have the advantages of low thermal conductivity and light weight, and the smooth spherical surface will not cause stress concentration at the interface and inside the matrix. If used to fill modified polymers, polymer composite materials with heat insulation, light weight and excellent mechanical properties can be prepared. However, hollow glass microspheres are directly filled into polymers as fillers. In the process, due to the great difference in polarity between it and the polymer, agglomeration is likely to occur, and the performance of the obtained material will be greatly reduced; in addition, polyurethane coils used outdoors, such as tracks and courts in outdoor sports venues, are prone to absorbing rain from the outside. Under the sun, the degradation and aging of the polyurethane coils will be accelerated, and the product will also turn yellow easily. Usually, ultraviolet absorbers and anti-aging agents are added during the product preparation process. However, these small molecule reagents are easy to precipitate on the surface of the material, and their effects are not long-lasting, and they cannot improve the problem of accelerated aging and yellowing of polyurethane coils due to rain in the long term. [Summary of the invention]
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a high-elasticity foamed polyurethane coil and a preparation method thereof.
[0005] The technical solution provided by the present invention can make up for the defects of the polyurethane coiled material provided by the prior art to a certain extent.
[0006] In order to achieve the above purpose, the following technical solutions are used:
[0007] A highly elastic foamed polyurethane coil, characterized in that the weight ratio of each raw material in parts by weight is:
[0008] High fluorine content polyol: 50-60 parts
[0009] Siliconized chain extender: 10-20 parts
[0010] Diphenylmethane diisocyanate: 30-40 parts
[0011] Modified hollow glass microspheres: 20-30 parts
[0012] Plasticizer: 10-15 parts
[0013] Antioxidant: 0.5-1 part
[0014] Catalyst: 0.1-1 parts
[0015] 3-Perfluorohexylpropanol: 10-20 parts
[0016] Triethylamine: 5-10 parts
[0017] Foaming agent: 0.5-2 parts
[0018] Foam stabilizer: 0.1-1.
[0019] In a preferred technical solution, the plasticizer is one or more of triethyl phosphate, tributyl phosphate, and tri-isooctyl phosphate.
[0020] In a preferred technical solution, the antioxidant is one or more of antioxidant 1098, antioxidant 1726, and antioxidant 264.
[0021] In a preferred technical solution, the catalyst is dibutyltin dilaurate and / or an organic bismuth zinc metal catalyst.
[0022] In a preferred technical solution, the foaming agent is water; and the foam stabilizer is a silicone oil foam stabilizer.
[0023] Furthermore, the present invention also provides a method for preparing a high elasticity foamed polyurethane coil, comprising the following steps:
[0024] 1. Weigh the raw materials according to the above ratio, add the high fluorine-containing polyol into the reaction container, vacuum dehydrate at 100-110° C. for 1-2 hours, then reduce the temperature to 70-80° C., add the diphenylmethane diisocyanate and stir for 2-4 hours to obtain a mixture A;
[0025] 2. Slowly add the 3-perfluorohexylpropanol to the mixture A, stir and react at 80-100° C. for 2-3 hours, then add the siliconized chain extender, the modified hollow glass microspheres, the catalyst, the plasticizer and the antioxidant to the reaction container, continue to stir and react for 2-3 hours, then reduce the temperature to 50-60° C., add the triethylamine, the foam stabilizer and the foaming agent to the reaction container, and continue to stir for 0.5-1 hour to obtain the mixture B;
[0026] 3. Add the mixed material B in step 2 into a mold, and obtain a sheet after curing and / or maturing. Cut and roll the sheet to obtain a foamed polyurethane coil.
[0027] The preparation process of the siliconized chain extender is as follows: add γ-glycidyloxypropyltrimethoxysilane and 2,6-di-tert-butyl-p-cresol into a flask, slowly drop hydroxyethyl acrylate under stirring in an ice-water bath, stir and react for 1-2 hours after the dropwise addition, then raise the temperature to 35-45°C and continue stirring and reacting for 5-8 hours to obtain a crude siliconized chain extender product, then extract with deionized water 2-3 times to remove unreacted monomers, and then place at 60°C and under negative pressure to remove the solvent by rotary evaporation to obtain the siliconized chain extender.
[0028] In the preparation process of the siliconized chain extender, the molar ratio of γ-glycidyloxypropyltrimethoxysilane to hydroxyethyl acrylate is 1:2.2, wherein the mass fraction of 2,6-di-tert-butyl-p-cresol is 0.1%.
[0029] The preparation process of the high-fluorine-content polyol is as follows: add polybutylene adipate into a flask, add perfluoroazelaic acid under an inert atmosphere, evacuate at 70-80°C and 1.5-2kPa for 1-2 hours, then add sodium acetate, stir for 1 hour to stop the reaction and obtain the high-fluorine-content polyol.
[0030] The weight ratio of each raw material in the preparation of the above-mentioned high-fluorine-content polyol is: polybutylene adipate: 20-30 parts, perfluoroazelaic acid: 20-30 parts, sodium acetate: 0.5-1 part.
[0031] The preparation process of the modified hollow glass microspheres is as follows: first, hollow glass microspheres (HGM) are treated with an alkaline solution to modify the inner and outer surfaces with hydroxyl groups to obtain hydroxyl-containing hollow glass microspheres (HGM-OH), HGM-OH is put into a flask, and then propanol, diethylenetriamine, and silane coupling agent KH-550 are added to the flask, and the mixture is reacted at 50-70° C. under stirring conditions for 2-3 hours, and the emulsion is centrifuged and washed with deionized water for 2-3 times to obtain the modified hollow glass microspheres.
[0032] The beneficial effects of the present invention are:
[0033] 1. The addition of the hollow glass microspheres of the present invention can enhance the impact resistance of the coiled material, and also give the coiled material good sound absorption and heat insulation properties, reduce friction noise and the influence of external high temperature, and slow down the aging of the coiled material. The modified hollow glass microspheres are combined with the polyurethane elastomer through chemical bond grafting, so that it has good physical compatibility and coating effect, which can improve the performance of the hollow glass microspheres in polyurethane.
[0034] 2. The present invention adopts a high-fluorine-content polyol, and the fluorine content in the elastomer can be as high as 70% or more, so that the coil contains many CF bonds. The presence of a high content of CF bonds can improve the stability of the main chain and promote the improvement of the light aging resistance of the coil. On the other hand, it can significantly reduce the surface energy of the material, greatly improve the waterproof performance of the coil, and enhance the yellowing resistance of the coil. The present invention further uses 3-perfluorohexylpropanol to unilaterally end-cap the prepolymer, thereby introducing a fluorocarbon group at the end of the polyurethane main chain. Since the fluorocarbon end group has a tendency to spontaneously migrate and enrich to the surface, the surface of the coil can be effectively protected, and the surface energy of the coil can be further reduced, and the water resistance and yellowing resistance of the coil can be improved.
[0035] 3. The present invention adopts a siliconized chain extender, introduces silicon into the main chain or side chain of the chain extender, and then extends the polyurethane prepolymer, and finally introduces silicon into the polyurethane chain, which can further improve the mechanical and high temperature resistance of the polyurethane coil and reduce the impact of outdoor high temperature on the product.
[0036] Additional aspects and advantages of the present invention will be given in part in the following description, will become apparent from the following description, or may be learned through embodiments of the present invention. [Specific implementation method]
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Other embodiments obtained by those skilled in the art without making any creative ideas belong to the scope of protection of the present invention.
[0038] The raw materials used in the examples and comparative examples of the present invention are all commercially available conventional industrial products except for those produced by the manufacturer.
[0039] Embodiment 1:
[0040] A highly elastic foamed polyurethane coil, characterized in that the weight ratio of each raw material in parts by weight is:
[0041] High fluorine content polyol: 50 parts
[0042] Siliconized chain extender: 15 parts
[0043] Diphenylmethane diisocyanate: 35 parts
[0044] Modified hollow glass microspheres: 20 parts
[0045] Plasticizer: 15 parts
[0046] Antioxidant: 1 part
[0047] Catalyst: 0.6 parts
[0048] 3-Perfluorohexylpropanol: 12 parts
[0049] Triethylamine: 6 parts
[0050] Foaming agent: 1 part
[0051] Foam stabilizer: 0.5.
[0052] Wherein, the plasticizer is triethyl phosphate, the antioxidant is antioxidant 1098, the catalyst is dibutyltin dilaurate, the foaming agent is water, and the foam stabilizer is a silicone oil foam stabilizer.
[0053] The preparation of the above-mentioned highly elastic foamed polyurethane coil comprises the following steps:
[0054] 1. Weigh the raw materials according to the above ratio, add the high-fluorine-content polyol into the reaction container, vacuum dehydrate at 110° C. for 2 hours, then reduce the temperature to 80° C., add the diphenylmethane diisocyanate and stir for 2-4 hours to obtain a mixture A;
[0055] 2. Slowly add the 3-perfluorohexylpropanol to the mixture A, stir and react at 100° C. for 2 h, then add the siliconized chain extender, the modified hollow glass microspheres, the catalyst, the plasticizer and the antioxidant to the reaction container, continue to react under stirring for 3 h, then reduce the temperature to 50° C., add the triethylamine, the foam stabilizer and the foaming agent to the reaction container, and continue to stir for 1 h to obtain the mixture B;
[0056] 3. Add the mixed material B in step 2 into a mold, solidify and / or mature it to obtain a sheet, and cut and roll the sheet to obtain a foamed polyurethane coil.
[0057] The preparation process of the siliconized chain extender is as follows: add γ-glycidyloxypropyltrimethoxysilane and 2,6-di-tert-butyl-p-cresol into a flask, slowly drop hydroxyethyl acrylate under stirring in an ice-water bath, stir and react for 1 hour after the dropwise addition, then raise the temperature to 35°C and continue stirring and reacting for 5 hours to obtain a crude siliconized chain extender product, then extract with deionized water three times to remove unreacted monomers, and then place at 60°C and negative pressure conditions to remove the solvent by rotary evaporation to obtain the siliconized chain extender.
[0058] In the preparation process of the siliconized chain extender, the molar ratio of γ-glycidyloxypropyltrimethoxysilane to hydroxyethyl acrylate is 1:2.2, wherein the mass fraction of 2,6-di-tert-butyl-p-cresol is 0.1%.
[0059] The preparation process of the high-fluorine-content polyol is as follows: polybutylene adipate is added to a flask, perfluoroazelaic acid is added under an inert atmosphere, vacuum is applied at 80°C and 2kPa for 2h, sodium acetate is added, and the reaction is stopped by stirring for 1h to obtain the high-fluorine-content polyol.
[0060] The weight ratio of each raw material in the preparation of the above-mentioned high-fluorine-content polyol is: polybutylene adipate: 30 parts, perfluoroazelaic acid: 30 parts, sodium acetate: 0.5 parts.
[0061] The preparation process of the modified hollow glass microspheres is as follows: first, the hollow glass microspheres (HGM) are treated with an alkaline solution to modify the inner and outer surfaces with hydroxyl groups to obtain hydroxyl-containing hollow glass microspheres (HGM-OH), the HGM-OH is put into a flask, and then propanol, diethylenetriamine, and silane coupling agent KH-550 are added to the flask, and the reaction is carried out at 70° C. under stirring conditions for 3 hours, and the emulsion is centrifuged and washed twice with deionized water to obtain the modified hollow glass microspheres.
[0062] Embodiment 2:
[0063] A highly elastic foamed polyurethane coil, characterized in that the weight ratio of each raw material in parts by weight is:
[0064] High fluorine content polyol: 60 parts
[0065] Siliconized chain extender: 12 parts
[0066] Diphenylmethane diisocyanate: 38 parts
[0067] Modified hollow glass microspheres: 25 parts
[0068] Plasticizer: 13 parts
[0069] Antioxidant: 1 part
[0070] Catalyst: 0.5 parts
[0071] 3-Perfluorohexylpropanol: 18 parts
[0072] Triethylamine: 6 parts
[0073] Foaming agent: 1.5 parts
[0074] Foam stabilizer: 0.8.
[0075] Among them, the plasticizer is triisooctyl phosphate, the antioxidants are antioxidant 1726 and antioxidant 264, the catalyst is an organic bismuth zinc metal catalyst, the foaming agent is water, and the foam stabilizer is a silicone oil foam stabilizer.
[0076] The preparation of the above-mentioned highly elastic foamed polyurethane coil comprises the following steps:
[0077] 1. Weigh the raw materials according to the above ratio, add the high fluorine-containing polyol into the reaction container, vacuum dehydrate at 100° C. for 1 hour, then reduce the temperature to 75° C., add the diphenylmethane diisocyanate and stir for 3 hours to obtain a mixture A;
[0078] 2. Slowly add the 3-perfluorohexylpropanol to the mixture A, stir and react at 90° C. for 2 h, then add the siliconized chain extender, the modified hollow glass microspheres, the catalyst, the plasticizer and the antioxidant to the reaction container, continue to stir and react for 3 h, then reduce the temperature to 60° C., add the triethylamine, the foam stabilizer and the foaming agent to the reaction container, and continue to stir for 0.5 h to obtain the mixture B;
[0079] 3. Add the mixed material B in step 2 into a mold, and obtain a sheet after curing and / or maturing. Cut and roll the sheet to obtain a foamed polyurethane coil.
[0080] The preparation process of the siliconized chain extender is as follows: γ-glycidyloxypropyltrimethoxysilane and 2,6-di-tert-butyl-p-cresol are added into a flask, hydroxyethyl acrylate is slowly added dropwise under stirring in an ice-water bath, and the mixture is stirred and reacted for 2 hours after the addition is completed. The temperature is then raised to 45° C. and the stirring reaction is continued for 8 hours to obtain a crude siliconized chain extender product. The unreacted monomers are then extracted three times with deionized water, and the mixture is then placed at 60° C. and under negative pressure to remove the solvent by rotary evaporation to obtain the siliconized chain extender.
[0081] In the preparation process of the siliconized chain extender, the molar ratio of γ-glycidyloxypropyltrimethoxysilane to hydroxyethyl acrylate is 1:2.2, wherein the mass fraction of 2,6-di-tert-butyl-p-cresol is 0.1%.
[0082] The preparation process of the high-fluorine-content polyol is as follows: polybutylene adipate is added to a flask, perfluoroazelaic acid is added under an inert atmosphere, vacuum is applied at 80°C and 1.5 kPa for 1 hour, sodium acetate is added, and the reaction is stopped by stirring for 1 hour to obtain the high-fluorine-content polyol.
[0083] The weight ratio of each raw material in the preparation of the above-mentioned high-fluorine-content polyol is: polybutylene adipate: 25 parts, perfluoroazelaic acid: 28 parts, sodium acetate: 0.5 parts.
[0084] The preparation process of the modified hollow glass microspheres is as follows: first, the hollow glass microspheres (HGM) are treated with an alkaline solution to modify the inner and outer surfaces with hydroxyl groups to obtain hydroxyl-containing hollow glass microspheres (HGM-OH), the HGM-OH is put into a flask, and then propanol, diethylenetriamine, and silane coupling agent KH-550 are added to the flask, and the reaction is carried out at 70° C. under stirring conditions for 3 hours, and the emulsion is centrifuged and washed twice with deionized water to obtain the modified hollow glass microspheres.
[0085] Example 3
[0086] A highly elastic foamed polyurethane coil, characterized in that the weight ratio of each raw material in parts by weight is:
[0087] High fluorine content polyol: 50 parts
[0088] Siliconized chain extender: 15 parts
[0089] Diphenylmethane diisocyanate: 35 parts
[0090] Modified hollow glass microspheres: 25 parts
[0091] Plasticizer: 12 parts
[0092] Antioxidant: 0.8 parts
[0093] Catalyst: 0.5 parts
[0094] 3-Perfluorohexylpropanol: 16 parts
[0095] Triethylamine: 7 parts
[0096] Foaming agent: 2 parts
[0097] Foam stabilizer: 0.6.
[0098] Wherein, the plasticizer is tributyl phosphate, the antioxidant is antioxidant 1098, the catalyst is dibutyltin dilaurate, the foaming agent is water, and the foam stabilizer is a silicone oil foam stabilizer.
[0099] The preparation of the above-mentioned highly elastic foamed polyurethane coil comprises the following steps:
[0100] 1. Weigh the raw materials according to the above ratio, add the high-fluorine-content polyol into the reaction container, vacuum dehydrate at 105° C. for 2 hours, then reduce the temperature to 80° C., add the diphenylmethane diisocyanate and stir for 4 hours to obtain a mixture A;
[0101] 2. Slowly add the 3-perfluorohexylpropanol to the mixture A, stir and react at 85° C. for 3 h, then add the siliconized chain extender, the modified hollow glass microspheres, the catalyst, the plasticizer and the antioxidant to the reaction container, continue to stir and react for 3 h, then reduce the temperature to 60° C., add the triethylamine, the foam stabilizer and the foaming agent to the reaction container, and continue to stir for 1 h to obtain the mixture B;
[0102] 3. Add the mixed material B in step 2 into a mold, and obtain a sheet after curing and / or maturing. Cut and roll the sheet to obtain a foamed polyurethane coil.
[0103] The preparation process of the siliconized chain extender is as follows: add γ-glycidyloxypropyltrimethoxysilane and 2,6-di-tert-butyl-p-cresol into a flask, slowly drop hydroxyethyl acrylate under stirring in an ice-water bath, stir and react for 1 hour after the dropwise addition, then raise the temperature to 40°C and continue stirring and reacting for 8 hours to obtain a crude siliconized chain extender product, then extract with deionized water 3 times to remove unreacted monomers, and then place at 60°C and negative pressure conditions to remove the solvent by rotary evaporation to obtain the siliconized chain extender.
[0104] In the preparation process of the siliconized chain extender, the molar ratio of γ-glycidyloxypropyltrimethoxysilane to hydroxyethyl acrylate is 1:2.2, wherein the mass fraction of 2,6-di-tert-butyl-p-cresol is 0.1%.
[0105] The preparation process of the high-fluorine-content polyol is as follows: polybutylene adipate is added to a flask, perfluoroazelaic acid is added under an inert atmosphere, vacuum is applied at 80°C and 1.5 kPa for 2 hours, sodium acetate is added, and the reaction is stopped by stirring for 1 hour to obtain the high-fluorine-content polyol.
[0106] The weight ratio of each raw material in the preparation of the above-mentioned high-fluorine-content polyol is: polybutylene adipate: 20-30 parts, perfluoroazelaic acid: 30 parts, sodium acetate: 1 part.
[0107] The preparation process of the modified hollow glass microspheres is as follows: first, the hollow glass microspheres (HGM) are treated with an alkaline solution to modify the inner and outer surfaces with hydroxyl groups to obtain hydroxyl-containing hollow glass microspheres (HGM-OH), the HGM-OH is put into a flask, and then propanol, diethylenetriamine, and silane coupling agent KH-550 are added to the flask, and the reaction is carried out at 70° C. under stirring conditions for 3 hours, and the emulsion is centrifuged and washed twice with deionized water to obtain the modified hollow glass microspheres.
[0108] Comparative Example 1
[0109] A highly elastic foamed polyurethane coiled material, compared with Example 2, hollow glass microspheres are used instead of modified hollow glass microspheres, and the rest are the same as Example 2.
[0110] Comparative Example 2
[0111] A highly elastic foamed polyurethane coiled material, compared with Example 2, uses conventional chain extender ethylene glycol instead of siliconized chain extender, and the rest is the same as Example 2.
[0112] Comparative Example 3
[0113] A highly elastic foamed polyurethane coiled material, compared with Example 2, uses polybutylene adipate instead of high-fluorine-containing polyol, and the rest is the same as Example 2.
[0114] Comparative Example 4
[0115] A highly elastic foamed polyurethane coiled material, compared with Example 2, does not contain the 3-perfluorohexylpropanol, and the rest is the same as Example 2.
[0116] The elastic polyurethane coils prepared in Examples 1-3 and Comparative Examples 1-4 were tested as follows: tensile properties were tested according to GB / T1040.1-2006; impact properties were tested according to GB 36246-2018; yellowing resistance test was performed on the samples: the prepared coils were cut into two pieces of the same size and thickness as a sample and a comparison sample, one of which was placed in a HZ-3017 bulb-type yellowing resistance test box and illuminated under a 400W ultraviolet lamp. The distance between the sample and the bulb was 30 cm, and the temperature in the exposure box was about 60°C. After continuous illumination for one week, its yellowing resistance was observed, and its color was compared with that of the blank comparison sample on a gray color card; according to GB / T 2406.2-2009 for flame retardant performance test, and GB / T14833-2020 for harmful substances test. The product is tested for waterproof performance: the water contact angle is measured by JC2000D contact angle meter, the test water is ultrapure water, 5 points are tested for each sample, and the average value is taken.
[0117] Some test results are shown in Table 1 below:
[0118] Table 1 shows the performance test results of the product:
[0119]
[0120]
[0121] It can be seen from the test results in Table 1 above that the elastic polyurethane coils of Examples 1-3 have good tensile strength, impact absorption and vertical deformation, are not easy to crack, have excellent mechanical properties, are waterproof and anti-fouling, and have strong yellowing resistance. The finished elastic polyurethane coils prepared in Examples 1-3 have a smooth appearance without dark bubbles, no harmful substances are detected, and have good flame retardant properties, fully meet environmental protection requirements, and are suitable for promotion and use in the industry.
[0122] In Comparative Examples 1-3, although some product performance indicators can be kept qualified, the performance in terms of tensile strength, impact absorption, vertical deformation performance, waterproof and anti-fouling, aging resistance, etc. is far inferior to that of the present invention. In Comparative Example 1, hollow glass microspheres are used instead of modified hollow glass microspheres. Due to the large difference in polarity between hollow glass microspheres and polymers, agglomeration is likely to occur, and the mechanical properties of the obtained material will be greatly reduced. In Comparative Example 2, conventional chain extender ethylene glycol is used instead of siliconized chain extender, and the introduction of silicon is reduced, resulting in reduced mechanical and heat resistance of polyurethane coils; in Comparative Example 3, polybutylene adipate is used instead of high-fluorine-containing polyols, which greatly reduces the waterproof and yellowing resistance of the coils; it can be seen that the presence of a high content of CF bonds improves the stability of the main chain on the one hand, promotes the improvement of the light aging resistance of the coils, and on the other hand In terms of the above aspects, the surface energy of the material can be significantly reduced, the waterproof performance of the coiled material is greatly improved, and the yellowing resistance of the coiled material is enhanced; in Comparative Example 4, 3-perfluorohexylpropanol is not added, and its waterproof and yellowing resistance is reduced to a certain extent. Although high-fluorine-content polyol is used for synthesis, some fluorocarbon chains are not easy to migrate to the surface due to the influence of the chemical bond energy of the polyurethane main chain. The present invention further uses 3-perfluorohexylpropanol to unilaterally end-cap the prepolymer. Relative to the fluorocarbon segment in the main chain of the polyurethane molecule, 3-perfluorohexylpropanol is added to graft the fluorocarbon segment on the end of the polyurethane molecular chain. Since the fluorocarbon end group has a tendency to spontaneously migrate and enrich to the surface, the surface of the coiled material can be effectively protected, the surface energy of the coiled material can be further reduced, and the water and yellowing resistance of the coiled material can be improved.
[0123] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A high elastic polyurethane foam coil, characterized in that: The weight ratio of each raw material in parts by weight is: high fluorine-containing polyol: 50-60 parts, siliconized chain extender: 10-20 parts, diphenylmethane diisocyanate: 30-40 parts, modified hollow glass microspheres: 20-30 parts, plasticizer: 10-15 parts, antioxidant: 0.5-1 part, catalyst: 0.1-1 part, 3-perfluorohexylpropanol: 10-20 parts, triethylamine: 5-10 parts, foaming agent: 0.5-2 parts, foam stabilizer: 0.1-1.
2. The high elasticity foamed polyurethane coil according to claim 1, characterized in that: The preparation process of the high-fluorine-content polyol is as follows: polybutylene adipate is added to a flask, perfluoroazelaic acid is added under an inert atmosphere, vacuum is applied at 70-80° C. and 1.5-2 kPa for 1-2 hours, sodium acetate is added, and the reaction is stopped by stirring for 1 hour to obtain the high-fluorine-content polyol.
3. The high elasticity foamed polyurethane coiled material according to claim 2, characterized in that: The weight ratio of each raw material in the preparation process of the high-fluorine-content polyol is: polybutylene adipate: 20-30 parts, perfluoroazelaic acid: 20-30 parts, sodium acetate: 0.5-1 part.
4. The high elasticity foamed polyurethane coiled material according to claim 1, characterized in that: The preparation process of the siliconized chain extender is as follows: γ-glycidyloxypropyltrimethoxysilane and 2,6-di-tert-butyl-p-cresol are added into a flask, hydroxyethyl acrylate is slowly added dropwise under stirring in an ice-water bath, and after the addition is completed, the mixture is stirred and reacted for 1-2 hours, and then the temperature is raised to 35-45° C. and the mixture is stirred and reacted for 5-8 hours to obtain a crude siliconized chain extender product, and then unreacted monomers are removed by extraction with deionized water for 2-3 times, and then the mixture is placed at 60° C. and under negative pressure to remove the solvent by rotary evaporation to obtain the siliconized chain extender.
5. The high elasticity foamed polyurethane coiled material according to claim 4, characterized in that: During the preparation of the siliconized chain extender, the molar ratio of the γ-glycidyloxypropyltrimethoxysilane to the hydroxyethyl acrylate is 1:2.2, and the mass fraction of the 2,6-di-tert-butyl-p-cresol is 0.1%.
6. The high elasticity foamed polyurethane coiled material according to claim 1, characterized in that: The preparation process of the modified hollow glass microspheres is as follows: first, the hollow glass microspheres are treated with an alkaline solution to obtain hydroxyl-containing hollow glass microspheres, the hydroxyl-containing hollow glass microspheres are placed in a flask, propanol, diethylenetriamine, and silane coupling agent KH-550 are added to the flask, and the mixture is reacted for 2-3 hours under stirring conditions at 50-70° C. to obtain an emulsion, and the emulsion is centrifuged and washed with deionized water for 2-3 times to obtain the modified hollow glass microspheres.
7. The high elasticity foamed polyurethane coiled material according to claim 1, characterized in that: The plasticizer is one or more of triethyl phosphate, tributyl phosphate, and tri(2-ethylhexyl) phosphate.
8. The high elasticity foamed polyurethane coiled material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1098, antioxidant 1726, and antioxidant 264.
9. The high elasticity foamed polyurethane coiled material according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate and / or an organic bismuth zinc metal catalyst; the foaming agent is water; and the foam stabilizer is a silicone oil foam stabilizer.
10. A method for preparing a high elasticity foamed polyurethane coil as claimed in any one of claims 1 to 9, comprising the following steps:
1. Weigh the raw material components according to the component ratio in claim 1; add the high fluorine-containing polyol into a reaction container, vacuum dehydrate at 100-110° C. for 1-2 hours, then reduce the temperature to 70-80° C., add the diphenylmethane diisocyanate and stir for 2-4 hours to obtain a mixture A; 2. Slowly add the 3-perfluorohexylpropanol to the mixture A, stir and react at 80-100° C. for 2-3 hours, then add the siliconized chain extender, the modified hollow glass microspheres, the catalyst, the plasticizer and the antioxidant to the reaction container, continue to stir and react for 2-3 hours, then reduce the reaction temperature to 50-60° C., add the triethylamine, the foam stabilizer and the foaming agent to the reaction container, and continue to stir for 0.5-1 hour to obtain the mixture B; 3. Add the mixed material B in step 2 into the mold to obtain a sheet after curing and / or maturing, and cut and roll the sheet to obtain the high elastic foamed polyurethane coil.
Citation Information
Patent Citations
Polyurethane pavement material
CN106739346A
Foaming polyurethane coiled material for paving playground and preparation method of foaming polyurethane coiled material
CN116063652A
Cited By
Low-density floating-resistant polyurethane runway material and preparation method thereof
CN120842835A