Alkyd resin with anti-corrosion and damp-proof functions
By rationally preparing polyols, dibasic acid, monoacid, silica, graphene and other components in alkyd resins, it forms anti-corrosion and moisture-proof coatings, solving the problem of poor anti-corrosion and moisture-proof performance of alkyd resins and achieving faster drying And better waterproof and moisture-proof effect.
Patent Information
- Application Number
- CN202411267428.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
AI Technical Summary
Due to its production process and other factors, the existing alkyd resin has poor corrosion and moisture resistance, which leads to the coating being easily damp and moldy as time increases, and has poor hydrophobicity, and has a long drying time.
Alkyd resin is formed by mixing polyols, dibasic acid, monobasic acid, silica, graphene, diluents, methyl acrylate, ethanol and cosolvents in a certain proportion, and then mixing them in sequence during the production process. Adding diluents and co-solvents improves the uniformity and dispersion speed of the components and shortens the drying time. At the same time, silica and graphene form a corrosion-proof layer on the surface, and methyl acrylate and ethanol fuse to form a moisture-proof protective layer.
It significantly improves the anti-corrosion and moisture-proof performance of alkyd resin, shortens the drying time and construction cycle, and forms an environmentally friendly anti-corrosion and moisture-proof coating, avoiding the problem of paint falling off and mold.
Smart Images

Figure CN118978677A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resins, and in particular to an alkyd resin with anti-corrosion and moisture-proof functions. Background Art
[0002] Alkyd resin is an oil-modified polyester resin formed by condensation polymerization of polyols, dibasic acids and monobasic acids. Alkyd resins can be divided into three categories: drying, semi-drying and non-drying according to the number and structure of double bonds in fatty acid (or oil) molecules. After curing into a film, it has gloss and toughness, strong adhesion, and good wear resistance, weather resistance and insulation. Alkyd resin coatings made from alkyd resins have the characteristics of weather resistance, good adhesion, brightness, fullness, etc., and are easy to apply. However, the coating film is relatively soft and has poor water and alkali resistance. At the same time, alkyd resins can be mixed with other resins to form a variety of self-drying or drying enamels, primers, topcoats and varnishes with different properties. They are widely used in the coating of buildings such as bridges, as well as machinery, vehicles, ships, aircraft, instruments, etc.
[0003] However, due to the production process and other factors, the existing alkyd resin has poor anti-corrosion and moisture-proof properties, resulting in the coating prepared with alkyd resin as raw material being easily affected by moisture and mold over time, and having poor hydrophobicity, and the existing alkyd resin takes a long time to dry. Summary of the invention
[0004] The purpose of the present application is to provide an alkyd resin with anti-corrosion and moisture-proof functions to solve the problems raised in the above background technology.
[0005] To achieve the above-mentioned purpose, the present application provides the following technical scheme: an alkyd resin with anti-corrosion and moisture-proof functions, including an alkyd resin finished product, the raw materials of the alkyd resin finished product including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents, the alkyd resin finished product is prepared by mixing polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents in a certain proportion, the polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents are respectively calculated according to the following weight parts, the polyols are 50-60 parts, the dibasic acids are 80-100 parts, the monobasic acids are 60-80 parts, the silica is 20-30 parts, the graphene is 5-8 parts, the diluents are 100-120 parts, the methyl acrylate is 20-30 parts, the ethanol is 80-100 parts, and the cosolvents are 10-15 parts.
[0006] A production process of an alkyd resin with anti-corrosion and moisture-proof functions comprises the following steps:
[0007] S1: Preliminary preparation: prepare the raw materials required for resin preparation, including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and co-solvents, and prepare weighing equipment, measuring cylinders, reactors with temperature control functions, and stirring and mixing equipment required for raw material processing. There are multiple sets of measuring cylinders and stirring and mixing equipment.
[0008] S2: Preparation of raw materials: Weigh the polyols, dibasic acids, monobasic acids, silicon dioxide, graphene, diluents, methyl acrylate, ethanol, and cosolvents required for the preparation of the finished coatings through a weighing device or a measuring cylinder, and weigh them according to the relevant proportions of 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silicon dioxide, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents for use;
[0009] S3: Preliminary preparation of alkyd resin: polyol, dibasic acid and monobasic acid are added to a reactor for mixed reaction. During the reaction, the mixture is added to the reactor to 60-80 degrees Celsius, mixed and stirred for 20-30 minutes, and the reaction is continued for 2-3 hours after the mixing and stirring is completed. After the reaction is completed, a diluent is added, the temperature of the reactor is maintained, and the mixing and stirring is continued for 30 minutes, and the reaction is continued for 2 hours. After the reaction is completed, an alkyd resin is obtained;
[0010] S4: Subsequent preparation of alkyd resin: After the alkyd resin sampling is completed, the remaining alkyd resin is continued to be stored in the reactor, and then silica is poured into the reactor for mixing and stirring, and a portion of the co-solvent is poured at the same time. When the silica is fully mixed, graphene is poured into the reactor and continued to be mixed. After the graphene is fully mixed, the reactor is maintained at a certain temperature, and the alkyd resin continues to react in the reactor;
[0011] S5: Final preparation of alkyd resin: while the alkyd resin with added silica and graphene continues to react in the reactor, ethanol is added to methyl acrylate several times and mixed and stirred. While stirring, the remaining co-solvent is evenly added to the mixture of methyl acrylate and ethanol several times. After the three are fully mixed, the mixed liquid is added to the reactor several times and mixed with the alkyd resin. After the mixed liquid and the alkyd resin are fully mixed and continue to react, an anti-corrosion and moisture-proof alkyd resin can be obtained.
[0012] Preferably, the polyol is one or more of glycerol, pentaerythritol and trimethylolpropane. When more than one polyol is used to prepare the alkyd resin, the ratio of glycerol, pentaerythritol and trimethylolpropane is 1:1:1.
[0013] Preferably, the dibasic acid used in the production of the alkyd resin is phthalic anhydride, and the monobasic acid is one or more of fatty acid, benzoic acid, and rosin. When more than one monobasic acid is used in the preparation of the alkyd resin, the ratio of the fatty acid, benzoic acid, and rosin is 1:1:1.
[0014] Preferably, the diluent used in the preparation of the alkyd resin is gasoline or xylene, and the diluent is selected from gasoline or xylene, and a mixture of gasoline and xylene is not selected as the diluent.
[0015] Preferably, after the alkyd resin is initially prepared, a sample of the alkyd resin without adding silicon dioxide, graphene, methyl acrylate and ethanol is taken and stored separately for subsequent comparative experiments.
[0016] Preferably, when the co-solvent is used, it is divided into two parts, one part of the co-solvent is used for mixing silica, graphene and alkyd resin, and the other part of the co-solvent is used for mixing methyl acrylate and ethanol, wherein the ratio of the co-solvent used for mixing silica, graphene and alkyd resin to the co-solvent used for mixing methyl acrylate and ethanol is 2:1.
[0017] Preferably, when the silica and graphene are added to the alkyd resin for reaction, the temperature of the reactor needs to be maintained at 70 to 80 degrees Celsius. When the silica, graphene and alkyd resin are mixed and stirred, the graphene can only be added after the silica is added to the reactor and mixed and stirred at a stirring speed of 1500 to 2000 revolutions per minute for ten minutes. During the mixing process, the co-solvent and silica are added to the reactor at the same time.
[0018] Preferably, when the ethanol and methyl acrylate are added to the reactor, the temperature of the reactor should be maintained at 50-60 degrees Celsius. After the ethanol and methyl acrylate are added to the reactor, they need to be mixed and stirred at 2000-500 revolutions per minute for twenty minutes, and then the temperature of the reactor is maintained at around 70 degrees Celsius for 2-4 hours.
[0019] Preferably, the alkyd resin is divided into two groups for comparative experiments, one group is alkyd resin with added silica, graphene, methyl acrylate and ethanol, and the other group is alkyd resin without added silica, graphene, methyl acrylate and ethanol. The two groups of alkyd resins are respectively added with other substances to make coatings, and then the coatings are sprayed on the experimental wall, and relevant data are recorded, including the drying time of the coating, the waterproof and moisture-proof properties of the coating, and the anti-corrosion properties of the coating.
[0020] In summary, the technical effects and advantages of the present invention are as follows:
[0021] In the present invention, polyol, dibasic acid, monobasic acid, silicon dioxide, graphene, diluent, methyl acrylate, ethanol and cosolvent are mixed and configured in a certain proportion to form an alkyd resin prepared in a certain ratio. In the production process, various raw materials are classified and mixed in sequence, and diluent and cosolvent are added at the same time, so that the components in the alkyd resin are mixed more evenly. At the same time, ethanol is added to the alkyd resin as a dispersion medium to increase the dispersion speed of each raw material, and at the same time, the volatilization speed of the alkyd resin when used can be increased, the surface drying and actual drying time can be shortened, and the construction period can be shortened. At the same time, because silicon dioxide and graphene are contained in the alkyd resin, the two cooperate with each other to form an anticorrosive layer on the surface of the alkyd resin, which blocks harmful substances in the air and is non-toxic and harmless, and is more environmentally friendly. Finally, methyl acrylate and ethanol are fused, so that the components in the alkyd resin are dispersed more evenly, and a moisture-proof protective layer is formed at the same time, so that the paint is not easy to be damp and moldy. Methyl acrylate increases the adsorption capacity of the alkyd resin to avoid the paint falling off. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 A schematic diagram of the production process of an alkyd resin with anti-corrosion and moisture-proof functions proposed in this application;
[0024] Figure 2 This is a comparison chart of the relevant data of the coating made from the alkyd resin sample and the finished product proposed in this application. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1: Reference Figure 1An alkyd resin with anti-corrosion and moisture-proof functions shown in the figure includes an alkyd resin finished product, the raw materials of the alkyd resin finished product include polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents, and the alkyd resin finished product is prepared by mixing polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents in a certain proportion, and the polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents are respectively calculated in the following parts by weight: 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silica, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents.
[0027] A production process of an alkyd resin with anti-corrosion and moisture-proof functions comprises the following steps:
[0028] S1: Preliminary preparation: prepare the raw materials required for resin preparation, including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and co-solvents, and prepare weighing equipment, measuring cylinders, reactors with temperature control functions, and stirring and mixing equipment required for raw material processing. There are multiple sets of measuring cylinders and stirring and mixing equipment.
[0029] S2: Preparation of raw materials: The polyol, dibasic acid, monobasic acid, silicon dioxide, graphene, diluent, methyl acrylate, ethanol, and cosolvent required for the preparation of the finished coating are weighed by a weighing device or a measuring cylinder, and the weighing is completed according to the relevant proportions of 50 parts of polyol, 80 parts of dibasic acid, 60 parts of monobasic acid, 20 parts of silicon dioxide, 5 parts of graphene, 100 parts of diluent, 20 parts of methyl acrylate, 80 parts of ethanol, and 10 parts of cosolvent for use;
[0030] S3: Preliminary preparation of alkyd resin: polyol, dibasic acid and monobasic acid are added to a reactor for mixed reaction. During the reaction, the mixture is added to the reactor to 60-80 degrees Celsius, mixed and stirred for 20-30 minutes, and the reaction is continued for 2-3 hours after the mixing and stirring is completed. After the reaction is completed, a diluent is added, the temperature of the reactor is maintained, and the mixing and stirring is continued for 30 minutes, and the reaction is continued for 2 hours. After the reaction is completed, an alkyd resin is obtained;
[0031] S4: Subsequent preparation of alkyd resin: After the alkyd resin sampling is completed, the remaining alkyd resin is continued to be stored in the reactor, and then silica is poured into the reactor for mixing and stirring, and a portion of the co-solvent is poured at the same time. When the silica is fully mixed, graphene is poured into the reactor and continued to be mixed. After the graphene is fully mixed, the reactor is maintained at a certain temperature, and the alkyd resin continues to react in the reactor;
[0032] S5: Final preparation of alkyd resin: while the alkyd resin with added silica and graphene continues to react in the reactor, ethanol is added to methyl acrylate several times and mixed and stirred. While stirring, the remaining co-solvent is evenly added to the mixture of methyl acrylate and ethanol several times. After the three are fully mixed, the mixed liquid is added to the reactor several times and mixed with the alkyd resin. After the mixed liquid and the alkyd resin are fully mixed and continue to react, an anti-corrosion and moisture-proof alkyd resin can be obtained.
[0033] Example 2: Reference Figure 1 An alkyd resin with anti-corrosion and moisture-proof functions shown in the figure includes an alkyd resin finished product, the raw materials of the alkyd resin finished product include polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents, and the alkyd resin finished product is prepared by mixing polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents in a certain proportion, and the polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents are respectively calculated in the following parts by weight: 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silica, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents.
[0034] A production process of an alkyd resin with anti-corrosion and moisture-proof functions comprises the following steps:
[0035] S1: Preliminary preparation: prepare the raw materials required for resin preparation, including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and co-solvents, and prepare weighing equipment, measuring cylinders, reactors with temperature control functions, and stirring and mixing equipment required for raw material processing. There are multiple sets of measuring cylinders and stirring and mixing equipment.
[0036] S2: Preparation of raw materials: The polyol, dibasic acid, monobasic acid, silicon dioxide, graphene, diluent, methyl acrylate, ethanol, and cosolvent required for the preparation of the finished coating are weighed by a weighing device or a measuring cylinder, and the weighing is completed according to the relevant proportions of 55 parts of polyol, 90 parts of dibasic acid, 70 parts of monobasic acid, 25 parts of silicon dioxide, 6 parts of graphene, 110 parts of diluent, 25 parts of methyl acrylate, 90 parts of ethanol, and 12 parts of cosolvent for use;
[0037] S3: Preliminary preparation of alkyd resin: polyol, dibasic acid and monobasic acid are added to a reactor for mixed reaction. During the reaction, the mixture is added to the reactor to 60-80 degrees Celsius, mixed and stirred for 20-30 minutes, and the reaction is continued for 2-3 hours after the mixing and stirring is completed. After the reaction is completed, a diluent is added, the temperature of the reactor is maintained, and the mixing and stirring is continued for 30 minutes, and the reaction is continued for 2 hours. After the reaction is completed, an alkyd resin is obtained;
[0038] S4: Subsequent preparation of alkyd resin: After the alkyd resin sampling is completed, the remaining alkyd resin is continued to be stored in the reactor, and then silica is poured into the reactor for mixing and stirring, and a portion of the co-solvent is poured at the same time. When the silica is fully mixed, graphene is poured into the reactor and continued to be mixed. After the graphene is fully mixed, the reactor is maintained at a certain temperature, and the alkyd resin continues to react in the reactor;
[0039] S5: Final preparation of alkyd resin: while the alkyd resin with added silica and graphene continues to react in the reactor, ethanol is added to methyl acrylate several times and mixed and stirred. While stirring, the remaining co-solvent is evenly added to the mixture of methyl acrylate and ethanol several times. After the three are fully mixed, the mixed liquid is added to the reactor several times and mixed with the alkyd resin. After the mixed liquid and the alkyd resin are fully mixed and continue to react, an anti-corrosion and moisture-proof alkyd resin can be obtained.
[0040] Example 3: Reference Figure 1 An alkyd resin with anti-corrosion and moisture-proof functions shown in the figure includes an alkyd resin finished product, the raw materials of the alkyd resin finished product include polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents, and the alkyd resin finished product is prepared by mixing polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents in a certain proportion, and the polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents are respectively calculated in the following parts by weight: 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silica, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents.
[0041] A production process of an alkyd resin with anti-corrosion and moisture-proof functions comprises the following steps:
[0042] S1: Preliminary preparation: prepare the raw materials required for resin preparation, including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and co-solvents, and prepare weighing equipment, measuring cylinders, reactors with temperature control functions, and stirring and mixing equipment required for raw material processing. There are multiple sets of measuring cylinders and stirring and mixing equipment.
[0043] S2: Preparation of raw materials: Weigh the polyols, dibasic acids, monobasic acids, silicon dioxide, graphene, diluents, methyl acrylate, ethanol, and cosolvents required for the preparation of the finished coatings through a weighing device or a measuring cylinder, and weigh them according to the relevant proportions of 60 parts of polyols, 100 parts of dibasic acids, 80 parts of monobasic acids, 30 parts of silicon dioxide, 8 parts of graphene, 120 parts of diluents, 30 parts of methyl acrylate, 100 parts of ethanol, and 15 parts of cosolvents for use;
[0044] S3: Preliminary preparation of alkyd resin: polyol, dibasic acid and monobasic acid are added to a reactor for mixed reaction. During the reaction, the mixture is added to the reactor to 60-80 degrees Celsius, mixed and stirred for 20-30 minutes, and the reaction is continued for 2-3 hours after the mixing and stirring is completed. After the reaction is completed, a diluent is added, the temperature of the reactor is maintained, and the mixing and stirring is continued for 30 minutes, and the reaction is continued for 2 hours. After the reaction is completed, an alkyd resin is obtained;
[0045] S4: Subsequent preparation of alkyd resin: After the alkyd resin sampling is completed, the remaining alkyd resin is continued to be stored in the reactor, and then silica is poured into the reactor for mixing and stirring, and a portion of the co-solvent is poured at the same time. When the silica is fully mixed, graphene is poured into the reactor and continued to be mixed. After the graphene is fully mixed, the reactor is maintained at a certain temperature, and the alkyd resin continues to react in the reactor;
[0046] S5: Final preparation of alkyd resin: while the alkyd resin with added silica and graphene continues to react in the reactor, ethanol is added to methyl acrylate several times and mixed and stirred. While stirring, the remaining co-solvent is evenly added to the mixture of methyl acrylate and ethanol several times. After the three are fully mixed, the mixed liquid is added to the reactor several times and mixed with the alkyd resin. After the mixed liquid and the alkyd resin are fully mixed and continue to react, an anti-corrosion and moisture-proof alkyd resin can be obtained.
[0047] As a preferred implementation of this embodiment, the polyol is one or more of glycerol, pentaerythritol, and trimethylolpropane. When more than one polyol is used to prepare the alkyd resin, the ratio of glycerol, pentaerythritol, and trimethylolpropane is 1:1:1.
[0048] As a preferred implementation mode of this embodiment, the dibasic acid used in the production of the alkyd resin is phthalic anhydride, and the monobasic acid is one or more of fatty acid, benzoic acid, and rosin. When more than one monobasic acid is used in the preparation of the alkyd resin, the ratio of the fatty acid, benzoic acid, and rosin is 1:1:1.
[0049] As a preferred implementation of this embodiment, the diluent used in the preparation of the alkyd resin is gasoline or xylene, and the diluent is selected from gasoline or xylene, and a mixture of gasoline and xylene is not selected as the diluent.
[0050] As a preferred implementation of this embodiment, after the alkyd resin is initially prepared, a sample of the alkyd resin without adding silicon dioxide, graphene, methyl acrylate, and ethanol is taken and stored separately for subsequent comparative experiments.
[0051] As a preferred implementation manner of this embodiment, when the co-solvent is used, it is divided into two parts, one part of the co-solvent is used for mixing silica, graphene and alkyd resin, and the other part of the co-solvent is used for mixing methyl acrylate and ethanol, wherein the ratio of the co-solvent used for mixing silica, graphene and alkyd resin to the co-solvent used for mixing methyl acrylate and ethanol is 2:1.
[0052] As a preferred implementation mode of this embodiment, when the silica and graphene are added to the alkyd resin for reaction, the temperature of the reactor needs to be maintained at 70 to 80 degrees Celsius. When the silica, graphene and alkyd resin are mixed and stirred, the graphene can only be added after the silica is added to the reactor and mixed and stirred at a stirring speed of 1500 to 2000 revolutions per minute for ten minutes. During the mixing process, the co-solvent and silica are added to the reactor at the same time.
[0053] As a preferred implementation mode of this embodiment, when the ethanol and methyl acrylate are added to the reactor, the temperature of the reactor should be maintained at 50-60 degrees Celsius. After the ethanol and methyl acrylate are added to the reactor, they need to be mixed and stirred at 2000-500 revolutions per minute for twenty minutes, and then the temperature of the reactor is maintained at around 70 degrees Celsius for 2-4 hours.
[0054] As a preferred implementation manner of this embodiment, the alkyd resin is divided into two groups for comparative experiments, one group is alkyd resin with added silica, graphene, methyl acrylate, and ethanol, and the other group is alkyd resin without added silica, graphene, methyl acrylate, and ethanol. The two groups of alkyd resins are respectively added with other substances to make coatings, and then the coatings are sprayed on the experimental wall, and relevant data are recorded, including the drying time of the coating, the waterproof and moisture-proof properties of the coating, and the anti-corrosion properties of the coating.
[0055] Working principle of the present invention:
[0056] In the present invention, polyol, dibasic acid, monobasic acid, silicon dioxide, graphene, diluent, methyl acrylate, ethanol and cosolvent are mixed and configured in a certain proportion to form an alkyd resin prepared in a certain ratio. In the production process, various raw materials are classified and mixed in sequence, and diluent and cosolvent are added at the same time, so that the components in the alkyd resin are mixed more evenly. At the same time, ethanol is added to the alkyd resin as a dispersion medium to increase the dispersion speed of each raw material, and at the same time, the volatilization speed of the alkyd resin when used can be increased, the surface drying and actual drying time can be shortened, and the construction period can be shortened. At the same time, because silicon dioxide and graphene are contained in the alkyd resin, the two cooperate with each other to form an anticorrosive layer on the surface of the alkyd resin, which blocks harmful substances in the air and is non-toxic and harmless, and is more environmentally friendly. Finally, methyl acrylate and ethanol are fused, so that the components in the alkyd resin are dispersed more evenly, and a moisture-proof protective layer is formed at the same time, so that the paint is not easy to be damp and moldy. Methyl acrylate increases the adsorption capacity of the alkyd resin to avoid the paint falling off.
[0057] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An alkyd resin having anti-corrosion and moisture-proof functions, including an alkyd resin finished product, characterized in that: The raw materials of the alkyd resin finished product include polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents. The alkyd resin finished product is prepared by mixing polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents in a certain proportion. The polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and cosolvents are respectively calculated in the following parts by weight: 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silica, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents.
2. A production process of an alkyd resin with anti-corrosion and moisture-proof functions, applicable to an alkyd resin with anti-corrosion and moisture-proof functions as claimed in claim 1, characterized in that: The following steps are involved: S1: Preliminary preparation: prepare the raw materials required for resin preparation, including polyols, dibasic acids, monobasic acids, silica, graphene, diluents, methyl acrylate, ethanol, and co-solvents, and prepare weighing equipment, measuring cylinders, reactors with temperature control functions, and stirring and mixing equipment required for raw material processing. There are multiple sets of measuring cylinders and stirring and mixing equipment. S2: Preparation of raw materials: Weigh the polyols, dibasic acids, monobasic acids, silicon dioxide, graphene, diluents, methyl acrylate, ethanol, and cosolvents required for the preparation of the finished coatings through a weighing device or a measuring cylinder, and weigh them according to the relevant proportions of 50-60 parts of polyols, 80-100 parts of dibasic acids, 60-80 parts of monobasic acids, 20-30 parts of silicon dioxide, 5-8 parts of graphene, 100-120 parts of diluents, 20-30 parts of methyl acrylate, 80-100 parts of ethanol, and 10-15 parts of cosolvents for use; S3: Preliminary preparation of alkyd resin: polyol, dibasic acid and monobasic acid are added to a reactor for mixed reaction. During the reaction, the mixture is added to the reactor to 60-80 degrees Celsius, mixed and stirred for 20-30 minutes, and the reaction is continued for 2-3 hours after the mixing and stirring is completed. After the reaction is completed, a diluent is added, the temperature of the reactor is maintained, and the mixing and stirring is continued for 30 minutes, and the reaction is continued for 2 hours. After the reaction is completed, an alkyd resin is obtained; S4: Subsequent preparation of alkyd resin: After the alkyd resin sampling is completed, the remaining alkyd resin is continued to be stored in the reactor, and then silica is poured into the reactor for mixing and stirring, and a portion of the co-solvent is poured at the same time. When the silica is fully mixed, graphene is poured into the reactor and continued to be mixed. After the graphene is fully mixed, the reactor is maintained at a certain temperature, and the alkyd resin continues to react in the reactor; S5: Final preparation of alkyd resin: while the alkyd resin with added silica and graphene continues to react in the reactor, ethanol is added to methyl acrylate several times and mixed and stirred. While stirring, the remaining co-solvent is evenly added to the mixture of methyl acrylate and ethanol several times. After the three are fully mixed, the mixed liquid is added to the reactor several times and mixed with the alkyd resin. After the mixed liquid and the alkyd resin are fully mixed and continue to react, an anti-corrosion and moisture-proof alkyd resin can be obtained.
3. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 1, characterized in that: The polyol is one or more of glycerol, pentaerythritol and trimethylolpropane. When more than one polyol is used for preparing the alkyd resin, the ratio of glycerol, pentaerythritol and trimethylolpropane is 1:1:
1.
4. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 1, characterized in that: The dibasic acid used in the production of the alkyd resin is phthalic anhydride, and the monobasic acid is one or more of fatty acid, benzoic acid, and rosin. When more than one monobasic acid is used in the preparation of the alkyd resin, the ratio of the fatty acid, benzoic acid, and rosin is 1:1:
1.
5. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 1, characterized in that: The diluent used in the preparation of the alkyd resin is gasoline or xylene. The diluent is selected from gasoline or xylene, and a mixture of gasoline and xylene is not selected as the diluent.
6. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 2, characterized in that: After the alkyd resin is initially prepared, a sample of the alkyd resin without adding silicon dioxide, graphene, methyl acrylate, and ethanol is taken and stored separately for subsequent comparative experiments.
7. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 2, characterized in that: When the co-solvent is used, it is divided into two parts, one part of the co-solvent is used for mixing silica, graphene and alkyd resin, and the other part of the co-solvent is used for mixing methyl acrylate and ethanol, wherein the ratio of the co-solvent used for mixing silica, graphene and alkyd resin to the co-solvent used for mixing methyl acrylate and ethanol is 2:
1.
8. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 2, characterized in that: When the silica and graphene are added to the alkyd resin for reaction, the temperature of the reactor needs to be maintained at 70 to 80 degrees Celsius. When the silica, graphene and alkyd resin are mixed and stirred, the graphene can only be added after the silica is added to the reactor and mixed and stirred at a stirring speed of 1500 to 2000 revolutions per minute for ten minutes. During the mixing process, the cosolvent and silica are added to the reactor at the same time.
9. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 2, characterized in that: When the ethanol and methyl acrylate are added to the reactor, the temperature of the reactor should be maintained at 50-60 degrees Celsius. After the ethanol and methyl acrylate are added to the reactor, they need to be mixed and stirred at 2000-500 revolutions per minute for 20 minutes, and then the temperature of the reactor is maintained at around 70 degrees Celsius for 2-4 hours.
10. The production process of an alkyd resin with anticorrosion and moisture-proof functions according to claim 2, characterized in that: The alkyd resin was divided into two groups for comparative experiments, one group was alkyd resin with added silica, graphene, methyl acrylate and ethanol, and the other group was alkyd resin without added silica, graphene, methyl acrylate and ethanol. The two groups of alkyd resins were respectively added with other substances to make coatings, and then the coatings were sprayed on the experimental wall, and relevant data were recorded, including the drying time of the coating, the waterproof and moisture-proof properties of the coating, and the anti-corrosion properties of the coating.