Bio-based organic silicon rubber foam additive as well as preparation method and application thereof
By using bio-based silicone rubber foam additives in silicone rubber foaming systems, using its parental structure and polyhydroxy fragment characteristics, the gas escape and cell inhomogeneity caused by conventional foam stabilizers are solved, and the low number of cells is achieved Foam silicone rubber properties with specific gravity and high closed cell ratio.
Patent Information
- Application Number
- CN202411299270.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-19
AI Technical Summary
The emulsification ability of conventional foam stabilizers in existing silicone rubber foaming systems is weak, resulting in gas escape and uneven bubble cells, making it difficult to achieve foam silicone rubber with low specific gravity and high closed cell ratio.
Using bio-based silicone rubber foam additives, its molecular structure contains glycosylated silicone and polyhydroxy glycosylated fragments with amphiphilic structures, participate in the foaming reaction, and plays the dual effect of stabilizing foam and foaming agent, reducing silicone rubber Specific gravity promotes gas fusion and cell uniformity.
Effectively avoid gas escape, improve closed cell rate and rebound performance, and achieve a uniform cell structure. It is suitable for foam silicone rubber with low specific gravity.
Smart Images

Figure BDA0005047122620000021 
Figure BDA0005047122620000022 
Figure BDA0005047122620000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone rubber, and in particular to a bio-based organic silicone rubber foam additive and a preparation method and application thereof. Background Art
[0002] Silicone rubber is a linear polysiloxane with alternating silicon-oxygen bonds (Si-O) forming its main chain and organic groups (such as methyl, ethyl, vinyl, phenyl, trifluoropropyl, etc.) forming its side groups. Silicone foam rubber has the advantages of both organic and inorganic materials and is widely used in aerospace, rail transportation, new energy vehicles, electronics and electrical fields.
[0003] The foam stabilizers used in silicone foam rubber are mostly conventional polyether modified silicone oil, fluorocarbon and other surfactants. Such additives have weak emulsification ability or cannot effectively reduce the interfacial tension between the silicone rubber phase and the gas phase. When used in low-viscosity foam silicone rubber systems, bubbles are easily fused and enlarged, and gas escapes, thereby reducing the foaming ratio. The uniformity of the pores is poor, and in severe cases, the bubbles disappear completely, and the purpose of stabilizing the foam cannot be achieved. In addition, it is difficult to achieve a foam silicone rubber with a specific gravity of 0.2 or less using conventional foam stabilizers. The escape and fusion of gas during the foaming process of silicone materials is a key factor affecting product performance. A uniform and delicate pore structure is conducive to improving the performance of foam silicone.
[0004] In view of this, this application is filed. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a bio-based silicone rubber foam additive and a preparation method and application thereof. The bio-based silicone rubber foam additive is applied to a silicone foam silicone rubber system, which can avoid the escape of gas during the foaming process and promote the fusion of gas. At the same time, it plays the dual effect of a foam stabilizer and a foaming agent, effectively reducing the specific gravity of the foamed silicone rubber, promoting the formation of uniform bubbles, increasing the closed cell rate, and improving the rebound performance, and has broad application prospects.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A bio-based silicone rubber foam additive, the structural formula of which is shown in Formula I:
[0008]
[0009] In formula I, R1 is hydrogen or hydroxymethyl, R2, R3, and R4 are each independently hydrogen or hydroxyl, m is a positive integer ≥0, n is a positive integer ≥0, and n+m ≥0.
[0010] The bio-based organosilicon rubber foam additive of the present invention contains amphiphilic sugar-based organosilicon and polyhydroxy sugar-based fragments in its molecular structure, which can participate in the foaming reaction of silicone rubber, effectively reduce the specific gravity of silicone rubber, have excellent emulsification ability, can improve the compatibility of the formulation system, and improve the solubility between the components. The silicone fragments in the molecular structure can effectively improve the compatibility of sugar-based organosilicon with the silicone system. The bio-based organosilicon rubber foam additive is applied to the silicone foam silicone rubber system, can avoid the escape of gas during the foaming process, promote the fusion of gas, and play the dual effects of foam stabilizer and foaming agent, effectively reduce the specific gravity of the foamed silicone rubber, promote the formation of uniform pores, improve the closed cell rate, and improve the resilience, and has broad application prospects.
[0011] As a preferred embodiment of the present invention, 0≤n+m≤30, preferably 7≤n+m≤15.
[0012] The inventors of the present invention have found that by controlling 7≤n+m≤15, better foam stabilization and foaming effects can be achieved, the specific gravity of the foamed silicone rubber can be effectively reduced, the formation of uniform bubbles can be promoted, the closed cell rate can be increased, and the rebound performance can be improved. If the n+m value is too high, the foam stabilization effect is low and the foaming ratio is low; if n+m is too small, the compatibility in silicone is poor, which will also lead to performance degradation. Therefore, in the present invention, it is necessary to control 7≤n+m≤15.
[0013] As a preferred embodiment of the present invention, the bio-based silicone rubber foaming auxiliary agent includes at least one of the compounds shown below:
[0014]
[0015]
[0016] The present invention also provides a method for preparing a bio-based silicone rubber foam additive, comprising the following steps:
[0017] reacting allyl glucoside, hydrogen-containing silicone oil and a catalyst in a solvent, removing the solvent, and obtaining a bio-based silicone rubber foam additive;
[0018] The allyl glycoside includes at least one of allyl-α-D-pyranoglucoside, allyl-α-D-pyranomannoside, allyl-α-D-pyranoarabinoside and allyl-α-D-pyranoxyloside.
[0019] As a preferred embodiment of the present invention, the molar ratio of the allyl glycoside to the hydrogen-containing silicone oil is 1:(1-1.05); and / or
[0020] The solid-liquid ratio of the allyl glycoside to the solvent is 1 g: (4-20) mL; and / or
[0021] The mass of the catalyst accounts for 10 to 200 ppm of the total amount of allyl glycoside and hydrogen-containing silicone oil.
[0022] As a preferred embodiment of the present invention, the structural formula of the hydrogen-containing silicone oil is shown in Formula II:
[0023]
[0024] In formula II, m is a positive integer ≥0, n is a positive integer ≥0, and n+m ≥0.
[0025] As a preferred embodiment of the present invention, the reaction temperature is 65 to 85° C., and the reaction time is 1 to 8 hours.
[0026] As a preferred embodiment of the present invention, the solvent includes at least one of isopropanol, water, acetone, ethanol, methanol, N,N-dimethylformamide, acetonitrile, dimethyl sulfoxide, cyclopentane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene nitrate, ethylene carbonate, 1,4-butyrolactone, and dimethylacetamide.
[0027] As a preferred embodiment of the present invention, the catalyst includes at least one of chloroplatinic acid, dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, stannous octoate, dibutyltin acetylacetonate, tetrabutyl titanate, tetra-tert-butyl titanate, diisopropoxy diacetylacetonato titanium, and diisopropoxy diacetylacetoethyl titanium.
[0028] The present invention also provides an application of a bio-based organic silicon rubber foam additive in the preparation of organic silicon foam silicone rubber.
[0029] The present invention also provides an organic silicon foam silicone rubber, comprising component A and component B;
[0030] The component A comprises the following components in parts by weight: 450 to 500 parts of a first vinyl-terminated silicone oil, 200 to 300 parts of a first vinyl silicone oil, 50 to 80 parts of α, ω-dihydroxy polydimethylsiloxane, 180 to 220 parts of aluminum hydroxide, and 0.5 to 2 parts of a catalyst;
[0031] The component B comprises the following components in parts by weight: 80 to 120 parts of a second vinyl-terminated silicone oil, 50 to 100 parts of a second vinyl silicone oil, 400 to 500 parts of aluminum hydroxide, 0.4 to 1 part of an inhibitor, 20 to 40 parts of a first hydrogen-containing silicone oil, 300 to 400 parts of a second hydrogen-containing silicone oil, and 2 to 10 parts of a bio-based silicone rubber foam additive;
[0032] The bio-based organosilicon rubber foam additive is the bio-based organosilicon rubber foam additive described above.
[0033] As a preferred embodiment of the present invention, the amount of the bio-based silicone rubber foam additive is 4 to 8 parts.
[0034] As a preferred embodiment of the present invention, the first vinyl-terminated silicone oil has a viscosity of 500 to 2000 cp at 25°C and a vinyl-terminated content of 0.2 to 0.4 wt%;
[0035] The viscosity of the second vinyl-terminated silicone oil at 25° C. is 500 to 2000 cp, and the vinyl-terminated content is 0.2 to 0.4 wt %;
[0036] The first vinyl silicone oil has a viscosity of 500 to 2000 cp at 25° C. and a terminal vinyl content of 0.05 to 0.2 wt %;
[0037] The second vinyl silicone oil has a viscosity of 500 to 2000 cp at 25° C. and a terminal vinyl content of 0.05 to 0.2 wt %;
[0038] The first hydrogen-containing silicone oil has a viscosity of 20-300 cp at 25° C. and a hydrogen content of 1-2 wt %;
[0039] The second hydrogen-containing silicone oil has a viscosity of 10 to 100 cp at 25° C. and a hydrogen content of 0.02 to 0.1 wt %.
[0040] As a preferred embodiment of the present invention, the inhibitor includes at least one of divinyltetramethyldisiloxane and tetravinyltetramethylcyclotetrasiloxane.
[0041] The beneficial effects of the present invention are as follows: the bio-based organic silicone rubber foam additive of the present invention contains amphiphilic sugar-based organic silicone and polyhydroxy sugar-based fragments in its molecular structure, which can participate in the foaming reaction of silicone rubber, effectively reduce the specific gravity of silicone rubber, have excellent emulsification ability, can improve the compatibility of the formulation system, and improve the solubility between the components. The silicone fragments in the molecular structure can effectively improve the compatibility of sugar-based organic silicone with the silicone system. The bio-based organic silicone rubber foam additive is applied to the silicone foam silicone rubber system, can avoid the escape of gas during the foaming process, promote the fusion of gas, and play the dual effects of a foam stabilizer and a foaming agent, effectively reduce the specific gravity of the foamed silicone rubber, promote the formation of uniform bubbles, improve the closed cell rate, and improve the resilience, and has broad application prospects. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0043] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0044] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0045] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0046] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.
[0047] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0048] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0049] Example 1
[0050] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0051] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 155.4 ml of isopropanol and 33.0 g of dried allyl-D-pyranoglucoside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-pyranoglucoside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 199.8 g of side hydrogenated silicone oil (hydrogen content 0.075%) was added dropwise, and the addition time was 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours, and the solvent was removed by reduced pressure distillation (100°C, -0.095MPa, 30 minutes) to obtain a bio-based silicone rubber foam additive, which was recorded as ZJ-1.
[0052] The structural formula of the ZJ-1 is shown below:
[0053]
[0054] Example 2
[0055] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0056] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 140.4 ml of isopropanol and 33.0 g of dried allyl-α-D-pyranoside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-pyranoside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 177.6 g of side hydrogenated silicone oil (hydrogen content 0.084%) was added dropwise, and the addition time was 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours, and the solvent was removed by reduced pressure distillation (100°C, -0.095MPa, 30 minutes) to obtain a bio-based silicone rubber foam additive, which was recorded as ZJ-2.
[0057] The structural formula of the ZJ-2 is as follows:
[0058]
[0059] Example 3
[0060] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0061] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 152.2 ml of isopropanol and 28.5 g of dried allyl-α-D-arabinopyranoside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-arabinopyranoside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 199.8 g of side hydrogenated silicone oil (hydrogen content 0.075%) was added dropwise, and the addition time was 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours, and the solvent was removed by reduced pressure distillation (100°C, -0.095 MPa, 30 minutes) to obtain a bio-based organic silicone rubber foam additive, which was recorded as ZJ-3.
[0062] The structural formula of the ZJ-3 is as follows:
[0063]
[0064] Example 4
[0065] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0066] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 93 ml of isopropanol and 28.5 g of dried allyl-α-D-pyranose xyloside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-pyranose xyloside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 111 g of side hydrogenated silicone oil (hydrogen content 0.13%) was added dropwise for 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours. The solvent was removed by vacuum distillation (100°C, -0.095 MPa, 30 minutes) to obtain a bio-based organic silicone rubber foam additive, which was recorded as ZJ-4.
[0067] The structural formula of the ZJ-4 is shown below:
[0068]
[0069] Example 5
[0070] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0071] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 155.4 ml of isopropanol and 33.0 g of dried allyl-D-pyranoglucoside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-pyranoglucoside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 77.7 g of side hydrogenated silicone oil (hydrogen content 0.19%) was added dropwise for 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours. The solvent was removed by vacuum distillation (100°C, -0.095 MPa, 30 minutes) to obtain a bio-based organic silicone rubber foam additive, which was recorded as ZJ-5.
[0072] The structural formula of the ZJ-5 is as follows:
[0073]
[0074] Example 6
[0075] A method for preparing a bio-based silicone rubber foam additive comprises the following steps:
[0076] In a four-necked flask equipped with a thermometer, a dropping funnel, a mechanical stirrer, and a condenser, 155.4 ml of isopropanol and 33.0 g of dried allyl-D-pyranoglucoside were added in sequence, stirring was started, the temperature was raised to 60 degrees, stirring was dissolved, and then 40 ppm of chloroplatinic acid (relative to the total amount of allyl-α-D-pyranoglucoside and side hydrogenated silicone oil) was added, and stirring was performed for 1 hour. The temperature was raised to 80 degrees, and 233.1 g of side hydrogenated silicone oil (hydrogen content 0.064%) was added dropwise, and the addition time was 30 minutes. After the addition was completed, the temperature was raised to reflux for reaction for 4 hours. The temperature was raised to 90 degrees and distilled for 0.5 hours, and the solvent was removed by reduced pressure distillation (100°C, -0.095MPa, 30 minutes) to obtain a bio-based organic silicone rubber foam additive, which was recorded as ZJ-6.
[0077] The structural formula of the ZJ-6 is shown below:
[0078]
[0079] Example 7
[0080] A kind of organic silicon foam silicone rubber, the preparation method of which is as follows:
[0081] Component A: At room temperature, 477.5 parts by weight of 1000cp terminal vinyl silicone oil (0.32% vinyl content) at 25°C, 251.5 parts by weight of 1000cp vinyl silicone oil (0.12% vinyl content) at 25°C and 62.5 parts by weight of 1500cpα,ω-dihydroxy polydimethylsiloxane at 25°C were mixed, and dispersed for 15 minutes at -0.09MPa vacuum and 1000rpm. 190 parts by weight of aluminum hydroxide were added, and dispersed for 30 minutes at -0.09MPa and 1000rpm. Finally, 1.4 parts by weight of Custer catalyst were added, and dispersed for 10 minutes at 800rpm. The material was cooled and packaged.
[0082] Component B: At room temperature, add 96 parts by weight of terminal vinyl silicone oil with a viscosity of 1000cp at 25°C (vinyl content 0.32%) and 76 parts by weight of vinyl silicone oil with a viscosity of 1000cp at 25°C (vinyl content 0.12%), and disperse for 20 minutes under a vacuum of -0.09MPa and a rotation speed of 1000rpm. Add 440 parts by weight of aluminum hydroxide, disperse at -0.09 MPa, 800-1500 rpm for 30 minutes, then add 0.65 parts by weight of divinyltetramethyldisiloxane, 31 parts by weight of hydrogenated silicone oil with a viscosity of 20 cp at 25°C (hydrogen content of 1.6%) and 334 parts by weight of hydrogenated silicone oil with a viscosity of 50 cp at 25°C (hydrogen content of 0.05%), and disperse at 500 rpm for 10 minutes; finally, add 6 parts by weight of bio-based silicone rubber foam additive ZJ-1, disperse at 200 rpm for 10 minutes, and cool and discharge.
[0083] Example 8
[0084] The difference between Example 8 and Example 7 is that the amount of the bio-based silicone rubber foam additive ZJ-1 is 4 parts by weight, and the other parts are the same.
[0085] Example 9
[0086] The difference between Example 9 and Example 7 is that the amount of the bio-based silicone rubber foam additive ZJ-1 is 8 parts by weight, and the other contents are the same.
[0087] Example 10
[0088] The difference between Example 10 and Example 7 is that the amount of the bio-based silicone rubber foam additive ZJ-1 is 2 parts by weight, and the other aspects are the same.
[0089] Embodiment 11
[0090] The difference between Example 11 and Example 7 is that the amount of the bio-based silicone rubber foam additive ZJ-1 is 10 parts by weight, and the other aspects are the same.
[0091] Example 12
[0092] The difference between Example 12 and Example 7 is that an equal amount of bio-based organosilicon rubber foam additive ZJ-2 is used to replace the bio-based organosilicon rubber foam additive ZJ-1, and the other contents are the same.
[0093] Example 13
[0094] The difference between Example 13 and Example 7 is that an equal amount of bio-based organosilicon rubber foam additive ZJ-3 is used to replace the bio-based organosilicon rubber foam additive ZJ-1, and the other contents are the same.
[0095] Embodiment 14
[0096] The difference between Example 14 and Example 7 is that an equal amount of bio-based organosilicon rubber foam additive ZJ-4 is used to replace the bio-based organosilicon rubber foam additive ZJ-1, and the other contents are the same.
[0097] Embodiment 15
[0098] The difference between Example 15 and Example 7 is that an equal amount of bio-based organosilicon rubber foam additive ZJ-5 is used to replace the bio-based organosilicon rubber foam additive ZJ-1, and the other contents are the same.
[0099] Example 16
[0100] The difference between Example 16 and Example 7 is that an equal amount of bio-based organosilicon rubber foam additive ZJ-6 is used to replace the bio-based organosilicon rubber foam additive ZJ-1, and the other contents are the same.
[0101] Test example
[0102] This test example tests the properties of the organic silicon foam silicone rubber prepared in Examples 7 to 15. Component A and component B are mixed to prepare organic silicon foam silicone rubber and its properties are tested. The test results are shown in Table 1.
[0103] Density test standard: ASTM D792.
[0104] The compression set test standard is: ASTM D1056 (100°C 50%).
[0105] The closed porosity test standard is: GB / T10799-2008.
[0106] The oil penetration rate test standard is: ZOND METHOD.
[0107] Table 1
[0108]
[0109]
[0110] It can be seen from Table 1 that the bio-based silicone rubber foam additive of the present invention is applied to the silicone foam silicone rubber system, which can avoid the escape of gas during the foaming process and promote the fusion of gas, and at the same time play the dual effects of foam stabilizer and foaming agent, effectively reduce the specific gravity of the foamed silicone rubber, promote the formation of uniform bubbles, increase the closed cell rate, and improve the rebound performance.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A bio-based silicone rubber foam additive, It is characterized in that Its structural formula is shown in Formula I: In Formula I, R 1 is hydrogen or hydroxymethyl, R 2 , R 3 , R 4 Each is independently hydrogen or hydroxy, m is a positive integer ≥0, n is a positive integer ≥0, and n+m ≥0.
2. The bio-based silicone rubber foam additive according to claim 1, It is characterized in that 0≤n+m≤30, preferably 7≤n+m≤15.
3. The bio-based silicone rubber foam additive according to claim 1, It is characterized in that The bio-based silicone rubber foaming agent includes at least one of the following compounds:
4. The method for preparing the bio-based silicone rubber foam additive according to any one of claims 1 to 3, It is characterized in that The following steps are involved: reacting allyl glucoside, hydrogen-containing silicone oil and a catalyst in a solvent, removing the solvent, and obtaining a bio-based silicone rubber foam additive; The allyl glycoside includes at least one of allyl-α-D-pyranoglucoside, allyl-α-D-pyranomannoside, allyl-α-D-pyranoarabinoside and allyl-α-D-pyranoxyloside.
5. The method for preparing the bio-based silicone rubber foam additive according to claim 4, It is characterized in that The molar ratio of the allyl glycoside to the hydrogen-containing silicone oil is 1:(1-1.05); and / or The solid-liquid ratio of the allyl glycoside to the solvent is 1 g: (4-20) mL; and / or The mass of the catalyst accounts for 10 to 200 ppm of the total amount of allyl glycoside and hydrogen-containing silicone oil.
6. The method for preparing the bio-based silicone rubber foam additive according to claim 4, It is characterized in that The structural formula of the hydrogen-containing silicone oil is shown in Formula II: In formula II, m is a positive integer ≥0, n is a positive integer ≥0, and n+m ≥0.
7. The method for preparing the bio-based silicone rubber foam additive according to claim 4, It is characterized in that The reaction temperature is 65-85° C., and the reaction time is 1-8 hours.
8. Use of the bio-based silicone rubber foam additive according to any one of claims 1 to 3 in the preparation of silicone foam silicone rubber.
9. A silicone foam silicone rubber, It is characterized in that It includes component A and component B; The component A comprises the following components in parts by weight: 450 to 500 parts of a first vinyl-terminated silicone oil, 200 to 300 parts of a first vinyl silicone oil, 50 to 80 parts of α, ω-dihydroxy polydimethylsiloxane, 180 to 220 parts of aluminum hydroxide, and 0.5 to 2 parts of a catalyst; The component B comprises the following components in parts by weight: 80 to 120 parts of a second vinyl-terminated silicone oil, 50 to 100 parts of a second vinyl silicone oil, 400 to 500 parts of aluminum hydroxide, 0.4 to 1 part of an inhibitor, 20 to 40 parts of a first hydrogen-containing silicone oil, 300 to 400 parts of a second hydrogen-containing silicone oil, and 2 to 10 parts of a bio-based silicone rubber foam additive; The bio-based organosilicon rubber foam additive is the bio-based organosilicon rubber foam additive according to any one of claims 1 to 3.
10. The organic silicon foam silicone rubber according to claim 9, It is characterized in that The first vinyl-terminated silicone oil has a viscosity of 500-2000 cp at 25° C. and a vinyl-terminated content of 0.2-0.4 wt %; The viscosity of the second vinyl-terminated silicone oil at 25° C. is 500 to 2000 cp, and the vinyl-terminated content is 0.2 to 0.4 wt %; The first vinyl silicone oil has a viscosity of 500 to 2000 cp at 25° C. and a terminal vinyl content of 0.05 to 0.2 wt %; The second vinyl silicone oil has a viscosity of 500 to 2000 cp at 25° C. and a terminal vinyl content of 0.05 to 0.2 wt %; The first hydrogen-containing silicone oil has a viscosity of 20 to 300 cp at 25° C. and a hydrogen content of 1 to 2 wt %; The second hydrogen-containing silicone oil has a viscosity of 10 to 100 cp at 25° C. and a hydrogen content of 0.02 to 0.1 wt %.