Porous micro-pyramid structured PDMS film and preparation method thereof, and Ppy / PDMS conductive film and preparation method thereof
By introducing micro pyramid structure and pore structure into the PDMS film and combining Ppy conductive materials to form a Ppy/PDMS conductive film, the problem of insufficient sensitivity and detection limit of flexible pressure sensors is solved, and a sensor with high sensitivity and wide pressure range is realized. Simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202411050831.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing flexible pressure sensors have shortcomings in sensitivity and detection limits, which are difficult to meet the requirements of high sensitivity and wide detection range, and there are few researches on the reasonable design of the combined structure.
Using porous micro pyramid structure PDMS film and its preparation method, by introducing micro pyramid structure and pore structure into the PDMS film, and combining Ppy conductive material on it, forming Ppy/PDMS conductive film, increasing the conductive path and contact area, and improving Pressure sensitivity of the sensor.
Through the combination of micro-pyramid structure and porous structure, the geometric changes of the conductive electrode are improved, the pressure sensitivity and detection limit of the sensor are increased, and the stability of a wide pressure range and multiple compression and release cycles is achieved, simplifying the preparation process. Reduced costs.
Smart Images

Figure CN118978739A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials, and relates to a flexible conductive film, and specifically to a porous micro-pyramid structure PDMS film and a preparation method thereof, a Ppy / PDMS conductive film and a preparation method thereof. Background Art
[0002] In the past few decades, in order to prepare higher performance sensor devices, researchers have widely used various conductive materials and elastic materials to improve the performance of sensors by selecting more suitable materials. Currently, common conductive materials include polypyrrole (Ppy), polyaniline (PANI), carbon nanotubes, etc. Among them, polypyrrole has excellent biocompatibility, high stability, easy synthesis and preparation, and high conductivity, so it can be studied in this regard (Pang, AL, Arsad, A. & Ahmadipour, M. Synthesis and factor affecting on the conductivity of polypyrrole: a short review. Polymers for Advanced Technologies 32, 1428-1454, doi: 10.1002 / pat.5201 (2020).). In the selection of elastic materials, materials such as polydimethylsiloxane (PDMS), polyacrylamine (PAM) and polyurethane (PU) are usually more likely to be selected. Among them, polydimethylsiloxane (PDMS) is an elastic polymer with a silicon group. Its molecular main chain structure is mainly composed of repeating units (Si(CH3)2O). Due to its stable chemical properties, good thermal stability, excellent biocompatibility, flexibility, and repeated stretching, PDMS is widely used in the manufacture of flexible sensors (Zhou, H. et al. Stretchable piezoelectric energy harvesters and self-powered sensors for wearable and implantable devices. Biosensors and Bioelectronics 168, doi:10.1016 / j.bios.2020.112569(2020)). Traditional flexible pressure sensors have a simple structure and can be prepared by simply mixing a conductive fabric in an elastic element between two electrodes. However, this usually cannot achieve the requirement of high sensitivity. This is because according to the sensing mechanism of resistive sensors, when subjected to external force, the tunneling resistance of the conductive fabric changes, but the change in piezoresistivity caused by the change in the filling fabric alone cannot meet the requirements. Therefore, the development of resistive pressure sensors with high sensitivity and a wide detection range remains a challenge at this stage. In addition, although various conductive materials have been studied, the rational design of combined structures that play an important role in balancing the sensitivity and detection limit of resistive pressure sensors has rarely been studied. Summary of the invention
[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a porous micro-pyramid structure PDMS film and a preparation method thereof, a Ppy / PDMS conductive film and a preparation method thereof, and prepare a PDMS elastic film material by combining a micro-pyramid structure with a porous structure, and composite a Ppy conductive material on the basis of the PDMS elastic film material, introduce a pore conductive path on the basis of the surface conductive path, reduce the contact resistance, and improve the sensitivity of the porous sensor. At the same time, the micro-pyramid structure forms a spring-like compressible platform, forming a base for the conductive electrode, which can maximize the geometric changes caused by the conductive electrode being compressed, thereby improving the pressure sensitivity of the sensor.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A method for preparing a porous micro-pyramid structure PDMS film comprises the following steps:
[0006] Step 1, mixing the PDMS precursor and the curing agent in a mass ratio of 10:1 and stirring evenly to prepare a PDMS prepolymer;
[0007] Step 2: vacuum degassing the PDMS prepolymer, and then adding NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stirring the polymer so that the NaCl particles can be evenly dispersed in the PDMS prepolymer;
[0008] Step 3, spin-coating the mixed glue solution of PDMS and NaCl obtained in step 2 on a silicon wafer that has been etched in advance to prepare a surface micro-pyramid groove structure, and curing it in an oven at 80-100° C. for 1-2 hours to prepare a micro-pyramid structure PDMS film;
[0009] Step 4: Soak the film obtained in step 3 in hot water at 60-80° C. for 16-24 hours and then dry it to prepare a porous micro-pyramid structure PDMS film.
[0010] Preferably, the PDMS precursor described in step 1 is a two-component PDMS of vinyl polydimethylsiloxane and hydrogen polydimethylsiloxane, and the curing agent is a platinum catalyst.
[0011] Preferably, the stirring rate in step 1 and step 2 is 1000 rpm, and the stirring time is 30 min.
[0012] Preferably, the vacuum degassing treatment in step 2 is to evacuate to 0.098 kPa and maintain it for 20 minutes.
[0013] Preferably, the NaCl particles in step 2 are ground in a mortar and sieved with 100-mesh and 200-mesh sieves to obtain NaCl particles with a particle size of 75 to 150 μm.
[0014] Preferably, the drying in step 4 is performed by placing the product in an oven at 60° C. for 1 hour.
[0015] A porous micro-pyramid structure PDMS film prepared by the method as described above.
[0016] A method for preparing a Ppy / PDMS conductive film comprises the following steps:
[0017] 10g FeCl3 6H2O was dispersed in 20ml deionized water and stirred for 5min to mix evenly. Then 2.5ml pyrrole monomer was added. After stirring again to mix evenly, the porous micro-pyramid structure PDMS film was placed in the film and deposited at 4°C for 6h. The porous micro-pyramid structure Ppy / PDMS conductive film was then obtained after washing and drying.
[0018] The present invention also protects a Ppy / PDMS conductive film prepared by the method as described above.
[0019] Compared with the prior art, the present invention has the following technical effects:
[0020] The porous structure of the PDMS film of the present invention is prepared by a template removal process, and the porosity in the film is controlled by adjusting the size and content of template NaCl particles, and then the film is solidified on a silicon wafer with a micro-pyramid structure prepared by etching in advance to prepare the micro-pyramid structure in the film. The porous structure prepared by precipitation of salt particles has good pore interconnectivity, and the pore size and porosity thereof can be adjusted by controlling the salt particles. Due to the porous three-dimensional interconnected structure, the film can also inherit greater strain; the micro-pyramid structure is added to the film by spin coating on the pre-etched silicon wafer, and a compressible platform similar to a spring is provided when an external force is received, and these platforms are deposited to form the substrate of the conductive electrode, which can maximize the geometric change caused by the conductive electrode under pressure, thereby improving the pressure sensitivity of the sensor; the method is easier to operate and implement, simple to operate, and has a high repetition rate;
[0021] Furthermore, a layer of polypyrrole (Ppy) was in situ polymerized on the PDMS film by chemical oxidation to prepare a porous Ppy / PDMS conductive film with a micro-pyramid structure. The porous structure increases the channels for molecular diffusion in the film and the specific surface area of the film, thereby introducing additional pore resistance and increasing the conductive path of the film, which not only improves the mass transfer rate but also provides more active sites. When assembled into a flexible sensor, when it is subjected to external pressure, due to the presence of the micro-pyramid structure on the surface of the elastomer, it can more effectively activate the conductive path, and because of the presence of the internal pore channels, the contact area between the sensor and the outside world will increase sharply, resulting in a decrease in contact resistance, which will further improve its sensitivity and help achieve higher sensitivity and detection limit. In the flexible pressure sensor, the flexible pressure sensor based on the porous structure film of the Ppy / PDMS micro-pyramid structure will have a wide pressure range, high sensitivity and stability during multiple compression and release cycles.
[0022] The preparation method of the invention is simple and feasible, low in cost, and easy to repeat and industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a cross-sectional morphology of the porous micro-pyramid structure PDMS film prepared in Example 1;
[0024] Figure 2 The surface morphology of the porous micro-pyramid structure PDMS film prepared in Example 1;
[0025] Figure 3 A tensile stress-strain curve of a porous micro-pyramid structure PDMS film prepared in Example 1 with a strain of 10%-60%;
[0026] Figure 4 This is the maximum stress diagram of the porous micro-pyramid structure PDMS film prepared in Example 1;
[0027] Figure 5 The porous micro-pyramid structure PDMS film prepared in Example 1 has undergone 80 compression-release cycles at a strain of 30%;
[0028] Figure 6 The stress-strain relationship diagram of the porous micro-pyramid structure PDMS film, the pure PDMS film and the micro-pyramid structure PDMS film prepared in Example 1. DETAILED DESCRIPTION
[0029] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0030] The PDMS precursor and curing agent used in the following embodiments are SYLGARD184 silicone rubber produced by Dow Corning Corporation of the United States. The PDMS precursor is a two-component PDMS of vinyl polydimethylsiloxane and hydrogen polydimethylsiloxane, and the curing agent is a platinum catalyst.
[0031] Example 1
[0032] A method for preparing a porous micro-pyramid structure PDMS film comprises the following steps:
[0033] Step 1: Mix the PDMS precursor and the curing agent in a mass ratio of 10:1 and stir evenly to prepare a PDMS prepolymer; the stirring rate is 1000 rpm and the stirring time is 30 min;
[0034] Step 2: evacuate the PDMS prepolymer to 0.098 kPa and maintain it for 20 minutes to perform vacuum degassing treatment. After completion, add NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stir it so that the NaCl particles can be evenly dispersed in the PDMS prepolymer; the stirring rate is 1000 rpm, and the stirring time is 30 minutes; the NaCl particles are ground in a mortar, and the NaCl particles with a particle size of 75 to 150 μm are screened out with 100 mesh and 200 mesh sieves;
[0035] Step 3, spin-coating the mixed glue solution of PDMS and NaCl obtained in step 2 on the silicon wafer which has been etched in advance to prepare the surface micro-pyramid groove structure, and curing it in an oven at 80° C. for 2 h to prepare a micro-pyramid structure PDMS film;
[0036] Step 4: Soak the film obtained in step 3 in 80° C. hot water for 16 hours and then place it in an oven at 60° C. for 1 hour to prepare a porous micro-pyramid structure PDMS film.
[0037] Disperse 10g FeCl3 6H2O in 20ml deionized water, stir for 5min to mix evenly, then add 2.5ml pyrrole monomer, stir again to mix evenly, put into the above-mentioned porous micro-pyramid structure PDMS film and deposit at 4°C for 6h, then wash with deionized water 3 times, and then place in an oven at 60°C for 1h to obtain the porous micro-pyramid structure Ppy / PDMS conductive film.
[0038] The surface and side morphologies of the film prepared in Example 1 were observed by SEM, and the microscopic morphologies were as follows: Figure 1As shown in the figure, by introducing a large number of pore structures into the material, it introduces more pore resistance, thereby increasing the contact area and conductive path with the load, which helps to enhance its performance. And compared with PDMS films without any pore structure, due to the porous three-dimensional interconnected structure, the film can also inherit greater strain.
[0039] Figure 1 The surface morphology of the porous micro-pyramid structure PDMS film prepared in Example 1 is as follows: Figure 2 It can be seen that the surface of the film is covered with closely arranged micro-pyramid structures, which greatly increases the specific surface area of the film and provides more attachment points for the subsequent deposition of polypyrrole materials, thereby enhancing the conductive properties of the film; and, while introducing the micro-pyramid structure, the surface morphology of the film is changed, which will cause the film to produce more obvious deformation or response when subjected to external stimuli such as pressure and temperature, which can significantly improve the sensitivity of the sensor.
[0040] By introducing pore structure and micro-pyramid structure into the film at the same time, the channels for molecular diffusion in the film and the specific surface area of the film are increased, which not only improves the mass transfer rate but also provides more active sites; when assembled into a flexible sensor, when it is subjected to external pressure, due to the presence of the surface pattern of the elastomer, it can more effectively activate the conductive path, and because of the presence of the internal pore channel, the contact area between the sensor and the outside world will increase sharply, resulting in a decrease in contact resistance, which will further improve its sensitivity.
[0041] The mechanical properties of the porous micro-pyramid structure PDMS film prepared in Example 1 were tested using a universal tensile testing machine. Figure 3 As shown, after applying a large deformation of up to 60%, the film can still recover to its initial state with very small energy dissipation, which indicates that the film has excellent mechanical flexibility.
[0042] Under tensile strains ranging from 10% to 60%, the maximum stress of the PDMS film with microstructured porous structure is as follows Figure 4 As shown, from Figure 4 It can be seen that although the PDMS film with a microstructured porous structure basically shows a gradual increase in the entire strain range, this proves that the continuity of the film deformation is good. In addition, the stress value of the film can reach 2.9Mpa and 3.4Mpa under 50% and 60% tensile deformation, which provides a strong guarantee for the test range of subsequent sensors. The porous micro-pyramid structure PDMS film prepared in Example 1 was subjected to 80 compression and release cycle tests under 30% strain. Figure 5 As shown, from Figure 5 It can be seen that the curves basically overlap, the film shows excellent toughness and repeatability, and can completely recover to its original shape after stretching.
[0043] Example 2
[0044] A method for preparing a porous micro-pyramid structure PDMS film comprises the following steps:
[0045] Step 1: Mix the PDMS precursor and the curing agent in a mass ratio of 10:1 and stir evenly to prepare a PDMS prepolymer; the stirring rate is 1000 rpm and the stirring time is 30 min;
[0046] Step 2: evacuate the PDMS prepolymer to 0.098 kPa and maintain it for 20 minutes to perform vacuum degassing treatment. After completion, add NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stir it so that the NaCl particles can be evenly dispersed in the PDMS prepolymer; the stirring rate is 1000 rpm, and the stirring time is 30 minutes; the NaCl particles are ground in a mortar, and the NaCl particles with a particle size of 75 to 150 μm are screened out with 100 mesh and 200 mesh sieves;
[0047] Step 3, spin-coating the mixed glue solution of PDMS and NaCl obtained in step 2 on a silicon wafer that has been etched to prepare a surface micro-pyramid groove structure, and curing it in an oven at 100° C. for 1 h to prepare a micro-pyramid structure PDMS film;
[0048] Step 4: Soak the film obtained in step 3 in 60° C. hot water for 24 hours and then place it in an oven at 60° C. for drying for 1 hour to prepare a porous micro-pyramid structure PDMS film.
[0049] Disperse 10g FeCl3 6H2O in 20ml deionized water, stir for 5min to mix evenly, then add 2.5ml pyrrole monomer, stir again to mix evenly, put into the above-mentioned porous micro-pyramid structure PDMS film and deposit at 4°C for 6h, then wash with deionized water 3 times, and then place in an oven at 60°C for 1h to obtain the porous micro-pyramid structure Ppy / PDMS conductive film.
[0050] Example 3
[0051] A method for preparing a porous micro-pyramid structure PDMS film comprises the following steps:
[0052] Step 1: Mix the PDMS precursor and the curing agent in a mass ratio of 10:1 and stir evenly to prepare a PDMS prepolymer; the stirring rate is 1000 rpm and the stirring time is 30 min;
[0053] Step 2: evacuate the PDMS prepolymer to 0.098 kPa and maintain it for 20 minutes to perform vacuum degassing treatment. After completion, add NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stir it so that the NaCl particles can be evenly dispersed in the PDMS prepolymer; the stirring rate is 1000 rpm, and the stirring time is 30 minutes; the NaCl particles are ground in a mortar, and the NaCl particles with a particle size of 75 to 150 μm are screened out with 100 mesh and 200 mesh sieves;
[0054] Step 3, spin-coating the mixed glue of PDMS and NaCl obtained in step 2 on the silicon wafer which has been etched in advance to prepare the surface micro-pyramid groove structure, and curing it in an oven at 90° C. for 1.5 h to prepare a micro-pyramid structure PDMS film;
[0055] Step 4: Soak the film obtained in step 3 in 70° C. hot water for 20 hours and then place it in an oven at 60° C. for 1 hour to prepare a porous micro-pyramid structure PDMS film.
[0056] Disperse 10g FeCl3 6H2O in 20ml deionized water, stir for 5min to mix evenly, then add 2.5ml pyrrole monomer, stir again to mix evenly, put into the above-mentioned porous micro-pyramid structure PDMS film and deposit at 4°C for 6h, then wash with deionized water 3 times, and then place in an oven at 60°C for 1h to obtain the porous micro-pyramid structure Ppy / PDMS conductive film.
[0057] Comparative Example 1
[0058] A method for preparing a micro-pyramid structure PDMS film comprises the following steps:
[0059] Step 1: Mix the PDMS precursor and the curing agent in a mass ratio of 10:1 and stir evenly to prepare a PDMS prepolymer; the stirring rate is 1000 rpm and the stirring time is 30 min;
[0060] Step 2: Spin-coat the PDMS prepolymer onto a silicon wafer that has been etched to prepare a surface micro-pyramid groove structure, and cure it in an oven at 90° C. for 1.5 h to prepare a micro-pyramid structure PDMS film.
[0061] Comparative Example 2
[0062] A method for preparing a porous PDMS film comprises the following steps:
[0063] Step 1: Mix the PDMS precursor and the curing agent in a mass ratio of 10:1 and stir evenly to prepare a PDMS prepolymer; the stirring rate is 1000 rpm and the stirring time is 30 min;
[0064] Step 2: evacuate the PDMS prepolymer to 0.098 kPa and maintain it for 20 minutes to perform vacuum degassing treatment. After completion, add NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stir it so that the NaCl particles can be evenly dispersed in the PDMS prepolymer; the stirring rate is 1000 rpm, and the stirring time is 30 minutes; the NaCl particles are ground in a mortar, and the NaCl particles with a particle size of 75 to 150 μm are screened out with 100 mesh and 200 mesh sieves;
[0065] Step 3: Spin-coat the mixed glue solution of PDMS and NaCl obtained in step 2 onto a smooth silicon wafer, and cure it in an oven at 90° C. for 1.5 h to prepare a porous PDMS film.
[0066] In order to study the influence of porous structure and microstructure on mechanical properties, the stress-strain relationship of the films prepared in Example 1, Comparative Example 1 and Comparative Example 2 was tested. Figure 6 As shown in the figure, with the introduction of microstructure and pore structure in the film, the stress-strain curve gradually becomes flat, indicating that the elastic modulus of the prepared film gradually decreases. Under the same stress, the material will produce a greater strain, so it is easier to deform when receiving a deformation force, and thus may absorb more energy. Therefore, the porous microstructured PDMS film is expected to perform well in the subsequent application of flexible sensors.
Claims
1. A method for preparing a porous micro-pyramid structure PDMS film, characterized in that: The following steps are involved: Step 1, mixing the PDMS precursor and the curing agent in a mass ratio of 10:1 and stirring evenly to prepare a PDMS prepolymer; Step 2: vacuum degassing the PDMS prepolymer, and then adding NaCl particles to the polymer at a mass ratio of 1:0.5 between the PDMS prepolymer and the NaCl particles, and stirring the polymer so that the NaCl particles can be evenly dispersed in the PDMS prepolymer; Step 3, spin-coating the mixed glue solution of PDMS and NaCl obtained in step 2 on a silicon wafer that has been etched in advance to prepare a surface micro-pyramid groove structure, and curing it in an oven at 80-100° C. for 1-2 hours to prepare a micro-pyramid structure PDMS film; Step 4: Soak the film obtained in step 3 in hot water at 60-80° C. for 16-24 hours and then dry it to prepare a porous micro-pyramid structure PDMS film.
2. The method for preparing a porous micro-pyramid structure PDMS film according to claim 1, characterized in that: The PDMS precursor described in step 1 is a two-component PDMS of vinyl polydimethylsiloxane and hydrogen polydimethylsiloxane, and the curing agent is a platinum catalyst.
3. The method for preparing a porous micro-pyramid structure PDMS film according to claim 1, characterized in that: The stirring rate in step 1 and step 2 is 1000 rpm, and the stirring time is 30 min.
4. The method for preparing a porous micro-pyramid structure PDMS film according to claim 1, characterized in that: The vacuum degassing treatment described in step 2 is to evacuate to 0.098 kPa and maintain it for 20 minutes.
5. The method for preparing a porous micro-pyramid structure PDMS film according to claim 1, characterized in that: The NaCl particles in step 2 are ground in a mortar and then screened with 100-mesh and 200-mesh screens to obtain NaCl particles with a particle size of 75 to 150 μm.
6. The method for preparing a porous micro-pyramid structure PDMS film according to claim 1, characterized in that: The drying described in step 4 is to place it in an oven at 60° C. for 1 hour.
7. A porous micro-pyramid structure PDMS film prepared by the method according to any one of claims 1 to 6.
8. A method for preparing a Ppy / PDMS conductive film, characterized in that: The following steps are involved: Disperse 10g FeCl3 6H2O in 20ml deionized water, stir for 5min to mix evenly, then add 2.5ml pyrrole monomer, stir again to mix evenly, put into the porous micro-pyramid structure PDMS film of claim 7 and deposit at 4°C for 6h, then wash and dry to obtain the porous micro-pyramid structure Ppy / PDMS conductive film.
9. A Ppy / PDMS conductive film prepared by the method according to claim 8.
Citation Information
Patent Citations
Method for preparing patterned polypyrrole film based on in-situ wrinkling
CN105085908A
Double-electrode flexible sensor capable of simultaneously detecting and distinguishing temperature and pressure as well as preparation method and application thereof
CN111998965A
Flexible capacitive sensor as well as preparation method and application thereof
CN112067175A
Artificial intelligence-based non-face-to-face treatment method
KR1020230123247A
Cited By
Flexible breathable plant leaf moisture monitoring sensor as well as preparation method and application thereof
CN119574651A