Polypropylene composition as well as preparation method and application thereof
By using nano-bar alumina filling and optimization process in polypropylene, the problems of insufficient thermal conductivity and material strength reinforcement are solved, and efficient thermal conductivity and mechanical performance enhancement are achieved, which is suitable for electronic heat dissipation devices. Reduced production costs and dust problems.
Patent Information
- Application Number
- CN202411093867.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
In applications where high thermal conductivity is required, polypropylene has insufficient thermal conductivity and is difficult to meet the needs of electronic heat dissipation devices. At the same time, in traditional methods, modified carbon fibers have problems such as dust dissipation and uneven material properties during mass production.
Nanobar alumina is used as filler to optimize material ratio and process to build a thermal conductivity network, improve the thermal conductivity of polypropylene, and improve dispersion and processing performance through compatibility agents and lubricants to reduce friction and raw material losses.
It significantly improves the thermal conductivity and mechanical properties of polypropylene, reduces processing difficulty and production costs, avoids uneven material properties and dust dissipation, is suitable for large-scale mass production, and can produce non-black modified materials to meet different appearance needs.
Smart Images

Figure CN118978765A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to a polypropylene composition and a preparation method and application thereof. Background Art
[0002] Polypropylene (PP) is a thermoplastic polymer widely used in various industrial and daily products. Due to its excellent mechanical properties, chemical stability, heat resistance and electrical insulation, polypropylene has been widely used in packaging, automotive industry, household appliances, textiles and medical devices. In addition, polypropylene has good processability and low cost, making it one of the preferred materials in many manufacturing industries.
[0003] Although polypropylene has many advantages, in some specific applications, such as environments that require high thermal conductivity, polypropylene compositions often fail to meet the required requirements. For example, in electronic heat dissipation devices, as the integration of electronic components increases in the electronics industry, the heat dissipation problem becomes increasingly severe. If polypropylene can be used as a heat dissipation housing or heat conduction plate for electronic components, it must have high thermal conductivity to ensure the stable operation of the components. However, the thermal conductivity of ordinary polypropylene is low and it is difficult to meet this requirement.
[0004] Patent document number CN117903531A discloses a high thermal conductivity and low electrical conductivity long glass fiber reinforced polypropylene composite material and its preparation method. The high thermal conductivity and low electrical conductivity long glass fiber reinforced polypropylene composite material of the present invention is coated with graphene oxide (GO) / thermoplastic polypropylene (PP) emulsion solution on the surface of continuous glass fiber to make it have high thermal conductivity and low electrical conductivity. The components of the high thermal conductivity and low electrical conductivity long glass fiber reinforced polypropylene composite material of the present invention are respectively: 40 to 70 parts of polypropylene resin, 1 to 5 parts of graphene oxide (GO) / thermoplastic polypropylene (PP) emulsion solution, 20 to 60 parts of continuous glass fiber, 1 to 5 parts of compatibilizer, and 0.1 to 1 part of antioxidant. However, the thermal conductivity of this material is not improved much compared with conventional polypropylene, and it cannot meet the requirements of electronic heat dissipation devices.
[0005] Patent document No. CN117700874A discloses a thermally conductive polypropylene material for new energy vehicles and a preparation method thereof; a thermally conductive polypropylene material for new energy vehicles, comprising the following raw materials in parts by weight: 50-70 parts of polypropylene, 5-15 parts of beryllium oxide, 5-20 parts of modified carbon fiber, 3-10 parts of DCP compatibilizer, 0.2-2 parts of lubricant, 0.1-0.4 parts of antioxidant, 0.2-0.4 parts of β-nucleating agent, and 0.2-1 parts of auxiliary agent; its preparation method is: S1, weighing polypropylene, beryllium oxide, modified carbon fiber, DCP compatibilizer, lubricant, antioxidant, β-nucleating agent, and auxiliary agent, mixing and stirring evenly to obtain a mixture; S2, the mixture is extruded, cooled in a water tank, and pelletized to obtain a finished product; it has the advantages of good thermal conductivity and high mechanical strength. Although this material has extremely high thermal conductivity, the modified carbon fiber is prone to cause serious dust dispersion in the workshop and uneven properties of the prepared material during mass production. Due to the large loss of carbon fiber raw materials, it is not convenient for large-scale mass production and reducing production costs. Summary of the invention
[0006] The present invention provides a polypropylene composition and a preparation method and application thereof, which can solve the above application requirements.
[0007] In order to solve the above technical problems, one of the purposes of the present invention provides a polypropylene composition, comprising the following components in parts by weight: polypropylene: 65 parts to 86 parts; nano-strip alumina: 10 parts to 35 parts; compatibilizer: 2.5 parts to 5 parts; lubricant: 0.5 parts to 1.5 parts; other additives: 0 parts to 5 parts.
[0008] By adopting the above scheme, the inventors used a special filler, namely nano-strip alumina. In the application field of thermal conductivity enhancement of polypropylene materials, traditional methods often find it difficult to simultaneously meet the dual requirements of high thermal conductivity and material strength, which greatly limits its application in the fields of high-efficiency heat dissipation components, electronic packaging, etc. In response to this technical bottleneck, this scheme creatively introduces a key additive, nano-strip alumina, and successfully solves the problem of insufficient thermal conductivity and poor reinforcement effect of polypropylene materials by optimizing material ratios and processes. The core innovation of this technical scheme lies in the addition of nano-strip alumina. Compared with traditional granular or flaky fillers, the nano-strip structure has a higher aspect ratio. This special form can effectively build a thermal conductive network, so that heat is quickly conducted inside the material along the long axis direction of the nano-strip, thereby significantly improving the thermal conductivity of polypropylene. At the same time, the high specific surface area and interface interaction of nano-strip alumina not only enhance the bonding force between the filler and the polypropylene matrix, but also effectively disperse stress through its rigid structure, improve the mechanical properties and deformation resistance of polypropylene, and achieve dual reinforcement of plastic materials. In addition, 2.5 to 5 parts of compatibilizer are added to the solution to improve the dispersibility and compatibility of nano-strip aluminum oxide in polypropylene, ensure that the formation of the thermal conductive network is not hindered, and further improve the thermal conductivity efficiency. At the same time, the appropriate amount of 0.5 to 1.5 parts of lubricant can help improve the fluidity during processing, reduce friction, and improve production efficiency and product quality. As for other additives, the flexible addition amount of 0 to 5 parts provides more possibilities for formula adjustment to meet the specific needs of different application scenarios.
[0009] As a preferred embodiment, the polypropylene resin is random copolymer polypropylene.
[0010] As a preferred embodiment, the compatibilizer is at least one of polyethylene grafted maleic anhydride or polypropylene grafted maleic anhydride.
[0011] As a preferred embodiment, the surface of the nano-strip aluminum oxide is pre-treated with graphene.
[0012] As a preferred embodiment, other additives include 0.3-0.5 parts of β-crystal nucleating agent.
[0013] As a preferred embodiment, other additives include 1-2 parts of precipitated barium sulfate.
[0014] As a preferred embodiment, the lubricant is graphite oxide, and the lubricant is 1.5 parts by weight. As the lubricant of the above technical solution, there are conventional stearates and some small molecular wax materials, which play a role in improving the fluidity and demolding performance of plastic processing. However, as a preferred embodiment, the lubricant used is graphite oxide, and the lubricant is 1.5 parts by weight. In the injection molding process, the role of the lubricant is to reduce friction, reduce the viscosity of the melt, and promote melt flow. In a polypropylene composition with a high filling rate, the filler will increase the viscosity and flow resistance of the melt, resulting in an increase in the difficulty of processing the composition and a decrease in surface quality. Therefore, it is very important to select a suitable lubricant to improve the processing performance and surface quality of the composition. The special layered structure of graphite oxide can play a role in lubricating and dispersing nano-strip aluminum oxide, as well as improving the orientation of nano-strip aluminum oxide. However, the amount of graphite oxide added should be controlled within a certain range, and excessive addition will affect the surface quality of the injection molded part. At the same time, the addition of graphite oxide should be fully mixed and dispersed to avoid uneven surface textures and black particles.
[0015] As a preferred embodiment, other additives include 0.2-0.4 parts by weight of a phenolic primary antioxidant and 0.2-0.4 parts by weight of a phosphite secondary antioxidant.
[0016] In order to solve the above technical problems, the second purpose of the present invention provides a method for preparing a polypropylene composition, comprising the following steps: mixing polypropylene, a compatibilizer, and a lubricant to obtain a first premix; mixing nano-strip alumina and other additives to obtain a second premix; uniformly mixing the first premix and the second premix, adding them to an extrusion device, and performing melt blending and extrusion granulation, wherein the extrusion temperature of the extrusion device is 210°C-230°C to obtain a polypropylene composition.
[0017] In order to solve the above technical problems, the third object of the present invention is to provide an application of a polypropylene composition in the field of electronic heat dissipation devices.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The polypropylene composition of the present invention uses the technical solution of filling tiny gaps and holes in the polypropylene substrate with nano-strip aluminum oxide to effectively improve the mechanical strength and thermal conductivity of the composition, so that it can meet the application of the polypropylene composition in the field of electronic heat dissipation devices.
[0020] 2. The polypropylene composition of the present invention has highly efficient thermal conductivity enhancement through nano-strip aluminum oxide, which is easier to process than traditional carbon fiber and graphene. It will not cause serious dust dispersion in the workshop and uneven material properties, and the loss of raw materials used is small, which is convenient for large-scale mass production and reduces production costs.
[0021] 3. The polypropylene composition material provided by the present invention does not require the use of carbon materials such as carbon fiber. The injection-molded surface of the modified plastic is glossy and has no obvious defects. Non-black modified materials can be produced to meet the appearance requirements of injection-molded products in different colors. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope image of the homemade nano-strip aluminum oxide in the example;
[0023] Figure 2 This is a scanning electron microscope image of ordinary alumina in comparative example 1. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The following are the sources and types of raw materials used in the examples and comparative examples of the present application. Unless otherwise specified, the reagents were obtained from commercial sources.
[0026] 1. Polypropylene resin
[0027] Homopolymer polypropylene: model is PPH-T03, melt flow rate (230℃ / 2.16kg) is 3.0g / 10min, manufacturer is Sinochem Refining & Chemical.
[0028] Random copolymer polypropylene: model SM 198, melt flow rate (230°C / 2.16kg) is 1.6g / 10min, and the manufacturer is Lotte of South Korea.
[0029] 2. Compatibilizer
[0030] Polypropylene grafted maleic anhydride (PP-g-MAH): model 21E830, manufacturer is DuPont.
[0031] Polyethylene grafted maleic anhydride (PE-g-MAH): model is CMG5804, manufacturer is Jiayirong.
[0032] 3. Nano-strip aluminum oxide
[0033] self made.
[0034] 4. Additives or others
[0035] β-crystal nucleating agent: model is NP-328, manufacturer is Ji Haichuan.
[0036] Lubricant: zinc stearate, manufactured by Huijinchuan Chemical.
[0037] Phosphoric acid: The manufacturer is Yongsheng Chemical.
[0038] Graphite oxide: GO-823, manufactured by Shanghai Zhenzhun Biotechnology.
[0039] Graphene: SY-rGO-L, manufactured by Beijing Meiston Technology Development Co., Ltd.
[0040] Phenolic primary antioxidant: 1010, manufactured by BASF.
[0041] Phosphite auxiliary antioxidant: 168, manufactured by BASF.
[0042] Precipitated barium sulfate: 3000 mesh, manufacturer is Hongzhi New Materials.
[0043] The preparation method of nano-strip aluminum oxide is as follows:
[0044] Aluminum sulfate was dissolved in a beaker to a concentration of 100 g / L, and sodium hydroxide was dissolved to a concentration of 18 g / L, and then set aside. After adding 100 ml of bottom water to a 2000 ml beaker, 500 ml of aluminum sulfate solution and 500 ml of sodium hydroxide were taken respectively, stirring was started, and the two solutions were added to the beaker at the same time, dripped at a speed of 30 ml / min, and the pH was maintained at 4.0 during the process. After the two solutions were added, 20 wt% sodium hydroxide was added to adjust the pH to 7.5, and then placed in a hydrothermal reactor, hydrothermally heated at 120°C for 4 hours, then taken out, filtered and washed with water to obtain a filter cake, which was dried at 105°C. The dried sample was placed in a calcining furnace and calcined at 1100°C for 2 hours in an atmospheric atmosphere to obtain nano-strip alumina. The obtained nano-scale strip alumina scanning electron microscope image is as shown in Figure 1 As shown, the average particle size is 67 nm.
[0045] Examples 1-6
[0046] A polypropylene composition can be used in the field of electronic heat dissipation devices, including polypropylene, nano-strip aluminum oxide, a compatibilizer, a lubricant, a phenolic primary antioxidant 1010, and a phosphite secondary antioxidant 168. The content of each component is shown in Table 1. The preparation method includes the following steps:
[0047] (1) mixing polypropylene, a compatibilizer, and a lubricant to obtain a first premix;
[0048] (2) mixing the nano-strip aluminum oxide, the phenolic primary antioxidant 1010 and the phosphite secondary antioxidant 168 to obtain a second premix;
[0049] (3) Then, the first premix and the second premix are uniformly mixed and added into a twin-screw extruder, and after melt blending and extrusion granulation, the extrusion temperature of the twin-screw extruder is 210° C. to 230° C., the first section is 210° C., the second to fourth sections are 230° C., the fifth to eighth sections are 220° C., and the ninth section of the die head is 210° C. to obtain the polypropylene composition.
[0050] Table 1 - Content of each component in Examples 1-6 (parts)
[0051] Components Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Homopolymer Polypropylene 65 84 70 65 65 Random copolymer polypropylene 65 Nano-strip aluminum oxide 25 25 10 35 25 25 PP-g-MAH 5 2.5 4 1.3 1.3 PE-g-MAH 2.5 0.7 0.7 Calcium stearate 1 0.5 1 1 Graphite oxide 1.5 1.5 β-crystal nucleating agent 0.5 0.5 Phenolic primary antioxidant 0.2 0.4 0.2 0.2 0.2 0.2 Phosphite auxiliary antioxidant 0.2 0.4 0.2 0.2 0.2 0.2 Precipitated barium sulfate 2
[0052] Example 7
[0053] A polypropylene composition, wherein each step and the reagents and process parameters used in each step in the preparation method are the same as those in Example 5, except that the surface of the nano-strip aluminum oxide is pretreated with graphene, and the method is as follows: filtering the reaction mixture, washing it with water, re-slurrying it, adding 1.3 parts by weight of graphene, adjusting the pH value to 4.5-5.0, stirring it for 0.5h, and dehydrating and drying it to obtain the modified nano-strip aluminum oxide.
[0054] Comparative Example 1
[0055] A polypropylene composition, wherein each step, reagents used in each step, and process parameters in the preparation method are the same as those in Example 1, except that the filler is ordinary alumina. The scanning electron microscope image of the alumina is as follows Figure 2 shown.
[0056] Comparative Example 2
[0057] A polypropylene composition, wherein each step, reagents used in each step and process parameters in the preparation method are the same as those in Example 1, except that no compatibilizer is added.
[0058] Performance testing
[0059] 1. Tensile strength: tested in accordance with ISO 527-2-2016, with a tensile speed of 50 mm / min. The test results are shown in Table 2;
[0060] 2. Bending strength: Tested in accordance with ISO 178. The test results are shown in Table 2.
[0061] 3. Izod notch impact strength: tested in accordance with ISO180-2000 standard, the test results are shown in Table 2;
[0062] 4. Surface condition of injection molded parts: The prepared polypropylene composition material was used to respectively mold color plates, and the surface condition of the color plates was tested using a gloss tester. The higher the test value, the better the gloss and the smoother the surface. The test results are shown in Table 2.
[0063] 5. Thermal conductivity: The thermal conductivity of the board was tested according to the test standard GB / T 10294; the test results are shown in Table 2.
[0064] Table 2 - Performance test results of Examples 1-7 and Comparative Examples 1-2
[0065]
[0066]
[0067] Combined with the performance test results of the embodiment and the comparative example in Table 2, it can be seen that the present invention uses nano-strip alumina as a filler, as a strong polar nano-filler for filling, giving the role of reinforcing between the polymer chains of polypropylene, and at the same time, the nano-strip alumina can further increase the thermal conductivity of polypropylene, and its special structure has excellent thermal conductivity and reinforcing properties for the modified material, which can meet the application requirements of electronic heat dissipation devices. Compared with conventional carbon fiber and graphene modified materials, the modified material of the present invention has low processing difficulty, will not cause serious dust drifting in the workshop and uneven material properties, the raw material loss used is small, it is convenient for large-scale mass production and reducing production costs, and, compared with the processing of black carbon materials, the injection molding surface of the modified plastic is glossy and has no obvious defects, and non-black modified materials can be produced, which can meet the appearance requirements of different colors of injection molding products. Among them, the compatibilizer improves the dispersibility and compatibility of nano-strip alumina in polypropylene to ensure that the formation of the thermal conductive network is not hindered. If the addition of the compatibilizer is cancelled, the overall thermal conductivity of the material will be significantly reduced and cannot meet the use requirements.
[0068] From the comparison of the data of Examples 2 and 1, it can be seen that the use of random copolymerized polypropylene as the raw material is conducive to obtaining a material with higher impact strength.
[0069] From the data comparison of Example 4, it can be seen that increasing the content of nano-strip aluminum oxide is beneficial to improving the mechanical properties and thermal conductivity of the material at the same time, and can also improve the surface gloss of the material.
[0070] From the data comparison of Examples 5 and 1, it can be seen that when graphite oxide is used as a lubricant, it is beneficial to simultaneously improve the mechanical properties and thermal conductivity of the material, and also improve the surface gloss of the material. Moreover, by using a composite compatibilizer, the total amount of compatibilizer can be reduced, further reducing the cost of the material. The use of a β-crystal nucleating agent is beneficial to further improve the surface gloss of the material.
[0071] The uniformity of dispersion of nano-strip alumina in polypropylene is crucial to the performance of the final material. The addition of precipitated barium sulfate helps to improve the dispersion state of nano-alumina and reduce agglomeration through the interaction between its particles. From the data comparison of Examples 6 and 1, it can be seen that precipitated barium sulfate can be used as a dispersing aid for nano-alumina, and promotes the uniform distribution of nano-alumina in the polypropylene matrix through steric hindrance effect and charge stabilization. In addition, the interaction between barium sulfate and nano-alumina may also promote the interface bonding between the two and the polypropylene matrix, thereby enhancing the performance of the composite material as a whole.
[0072] As a two-dimensional material, graphene has a very high thermal conductivity. After the surface of nano-strip aluminum oxide is modified by a small amount of graphene, graphene can form a layer of graphene coating on the surface of aluminum oxide, thereby significantly improving the thermal conductivity of polypropylene composite materials. As can be seen from the data of Example 7, the thermal conductivity of the modified material has been significantly improved. The inventors believe that graphene pretreatment can improve the interfacial bonding force between nano-strip aluminum oxide and polypropylene matrix. The high specific surface area and excellent mechanical properties of graphene enable it to form a strong interaction with aluminum oxide and polypropylene, thereby enhancing the overall performance of the composite material. The improvement of interfacial bonding force helps to reduce interfacial slip and damage of the composite material during the stress process, and improves the strength and durability of the material.
[0073] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A polypropylene composition, characterized in that The composition comprises the following components in parts by weight: polypropylene: 65 parts to 86 parts; Nano-strip aluminum oxide: 10-35 parts; Compatibilizer: 2.5-5 parts; Lubricant: 0.5-1.5 parts; Other additives: 0-5 parts.
2. A polypropylene composition according to claim 1, characterized in that The polypropylene resin is random copolymer polypropylene.
3. A polypropylene composition according to claim 2, characterized in that: The compatibilizer is at least one of polyethylene grafted maleic anhydride or polypropylene grafted maleic anhydride.
4. A polypropylene composition according to claim 3, characterized in that: The surface of the nano-strip aluminum oxide is pre-treated with graphene.
5. A polypropylene composition according to claim 1, characterized in that: The other auxiliary agents include 0.3-0.5 parts of β-crystal nucleating agent.
6. A polypropylene composition according to claim 1, characterized in that: The other auxiliary agents include 1-2 parts of precipitated barium sulfate.
7. A polypropylene composition according to claim 1, characterized in that: The lubricant is graphite oxide, and the amount of the lubricant is 1.5 parts by weight.
8. A polypropylene composition according to claim 1, characterized in that: The other auxiliary agents include 0.2-0.4 parts by weight of a phenolic primary antioxidant and 0.2-0.4 parts by weight of a phosphite secondary antioxidant.
9. A method for preparing a polypropylene composition, characterized in that: Used to prepare a polypropylene composition as described in any one of claims 1 to 8, comprising the following steps: mixing polypropylene, a compatibilizer, and a lubricant to obtain a first premix; mixing nano-strip alumina and other additives to obtain a second premix; uniformly mixing the first premix and the second premix, adding them to an extrusion device, and performing melt blending and extrusion granulation, wherein the extrusion temperature of the extrusion device is 210° C.-230° C. to obtain a polypropylene composition.
10. Use of the polypropylene composition according to any one of claims 1 to 8 in the field of electronic heat dissipation devices.