High-strength PVC pipe and preparation method thereof

Through specific formulas and processing techniques, high-strength PVC pipes are prepared, which solves the problem of insufficient impact and tensile strength of PVC pipes and improves its corrosion resistance and mechanical properties.

CN118978774APending Publication Date: 2024-11-19XINJIANG HONGNIAO WATER SAVING MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411286706.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The impact strength and tensile strength of PVC pipes are poor, and there are internal stress, large shrinkage and weld mark defects, which affect their strength and internal quality.

Method used

Using polyvinyl chloride resin, modified nitrile rubber, ethylene-octene copolymer, filler, reinforcement fiber, lubricant and titanate coupling agent, through specific formulas and processing techniques, including high-speed stirring and cold mixing Twin screw extrusion molding to prepare high-strength PVC pipes.

Benefits of technology

It improves the corrosion resistance, impact resistance and tensile strength of PVC pipes, and enhances the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043294220000101
    Figure BDA0005043294220000101
  • Figure BDA0005043294220000103
    Figure BDA0005043294220000103
  • Figure BDA0005043294220000111
    Figure BDA0005043294220000111
Patent Text Reader

Abstract

The invention discloses a high-strength PVC (polyvinyl chloride) pipe and a preparation method thereof. The plastic is prepared from the following raw materials in parts by weight: 150-250 parts of polyvinyl chloride resin, 10-30 parts of modified nitrile rubber, 10-30 parts of an ethylene-octene copolymer, 15-25 parts of filler, 10-20 parts of reinforced fibers, 1-3 parts of a lubricant, 1-3 parts of a plasticizer and 1-4 parts of a titanate coupling agent. The high-strength PVC pipe provided by the invention has good corrosion resistance and high mechanical strength. The combined use of the modified nitrile rubber and the ethylene-octylene copolymer in the components improves the corrosion resistance of the material, the combined use of the paigeite powder and the molybdenite powder enhances the impact resistance of the material, and the combined use of the ceramic fibers and the long carbon nanotubes enhances the tensile strength and bending strength of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipe manufacturing, and particularly relates to a high-strength PVC pipe and a preparation method thereof. Background Art

[0002] PVC pipe is a common plastic pipe, widely used in construction, municipal administration, agriculture, chemical industry and other fields. The specifications and sizes of PVC water supply pipes are very diverse, ranging from Φ20 to Φ800, and the nominal pressures are 0.63Mpa, 0.8Mpa, 1.0Mpa, 1.25Mpa, 1.6Mpa and other specifications. PVC pipes have the advantages of light weight, excellent corrosion resistance, low fluid resistance, high mechanical strength, simple construction, low cost, and no effect on water quality. The production process of PVC pipes involves the preparation, mixing, extrusion molding of raw materials and additives, and finally becomes a finished product after cooling, cutting, testing and packaging. When choosing PVC pipes, you also need to consider its size specifications, temperature and pressure resistance, and whether it is suitable for specific application scenarios.

[0003] Although PVC pipes have many advantages, they also have some defects that need to be improved. The impact strength and tensile strength of PVC pipes are poor, which may be due to improper raw material formulation, poor mixing effect of the composite system or unreasonable setting of extrusion process parameters, resulting in poor plasticization. PVC pipes have residual internal stress, large shrinkage rate and weld mark defects, which may lead to reduced strength. Improper extrusion temperature control can cause surface defects of the pipe and affect the internal quality. Too high temperature may cause melt decomposition, while too low temperature may lead to poor plasticization. Wrinkles, cracks, black lines, cloud lines, these surface defects may be caused by improper adjustment of traction speed, impurities in raw materials or too low extrusion temperature. Summary of the invention

[0004] The object of the present invention is to provide a high-strength PVC pipe and a preparation method thereof.

[0005] A high-strength PVC pipe is made of the following raw materials in parts by weight: 150-250 parts of polyvinyl chloride resin, 10-30 parts of modified nitrile rubber, 10-30 parts of ethylene-octene copolymer, 15-25 parts of filler, 10-20 parts of reinforcing fiber, 1-3 parts of lubricant, 1-3 parts of plasticizer and 1-4 parts of titanate coupling agent.

[0006] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 5-15 parts of styrene and 3-8 parts of divinylbenzene are dissolved in 30-60 parts of N,N-dimethylformamide and stirred to mix evenly, 1-4 parts of nitrile rubber are added and stirred evenly, 0.1-0.3 parts of benzoyl peroxide are added, stirred and heated to 80-90° C. for reaction for 8-12 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N,N-dimethylformamide is removed and then the material is cut, and the modified nitrile rubber is obtained after drying.

[0007] The filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1.

[0008] The reinforcing fibers are a mixture of ceramic fibers and long carbon nanotubes in a mass ratio of 4:1.

[0009] The average length of the long carbon nanotubes is 200-1000 μm.

[0010] The lubricant is one or more of microcrystalline wax, stearic acid, polypropylene wax and polyethylene wax.

[0011] The plasticizer is one or more of di(2-ethylhexyl)phthalate, hydrogenated rosin, diisononyl phthalate, and diisodecyl phthalate.

[0012] The titanate coupling agent is one or more of tris(dioctylpyrophosphoryloxy)titanate isopropyl ester, tetraoctyloxytitanium [di(tridecyl phosphite)], and tetraoctyloxytitanium [di(dilauryl phosphite)].

[0013] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0014] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110-130° C., and stopping stirring to obtain a premix;

[0015] (2) The premix is ​​conveyed to a cold mixer for stirring and cooling to 35-50°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding.

[0016] The processing temperature of the twin-screw extruder is 170-190°C.

[0017] Beneficial effects of the present invention: The high-strength PVC pipe of the present invention has good anti-corrosion performance and high mechanical strength. The combination of modified nitrile rubber and ethylene-octene copolymer in the components improves the anti-corrosion performance of the material, the combination of boron iron ore powder and molybdenum calcium ore powder enhances the impact resistance of the material, and the combination of ceramic fiber and long carbon nanotube enhances the tensile strength and bending strength of the material. DETAILED DESCRIPTION

[0018] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0019] Example 1

[0020] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified nitrile rubber, 20 parts of ethylene-octene copolymer, 20 parts of filler, 15 parts of reinforcing fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; and the average length of the long carbon nanotubes is 500 μm.

[0021] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0022] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0023] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0024] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0025] Example 2

[0026] A high-strength PVC pipe is made of the following raw materials in parts by weight: 150 parts of polyvinyl chloride resin, 10 parts of modified nitrile rubber, 10 parts of ethylene-octene copolymer, 15 parts of filler, 10 parts of reinforcing fiber, 1 part of stearic acid, 1 part of hydrogenated rosin, and 1 part of tetraoctyloxytitanium [di(tridecylphosphite)]; the filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; the average length of the long carbon nanotubes is 300 μm.

[0027] The preparation method of the modified nitrile rubber is as follows: according to the weight ratio, 5 parts of styrene and 4 parts of divinylbenzene are dissolved in 30 parts of N, N-dimethylformamide and stirred to mix evenly, 2 parts of nitrile rubber are added and stirred evenly, 0.1 parts of benzoyl peroxide are added, stirred and heated to 80° C. to react for 12 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0028] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0029] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110° C., and then stopping stirring to obtain a premix;

[0030] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 35° C., then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 170° C.

[0031] Example 3

[0032] A high-strength PVC pipe is made of the following raw materials in parts by weight: 250 parts of polyvinyl chloride resin, 30 parts of modified nitrile rubber, 30 parts of ethylene-octene copolymer, 25 parts of filler, 20 parts of reinforcing fiber, 3 parts of polyethylene wax, 3 parts of diisononyl phthalate, and 4 parts of tetraoctyloxytitanium [di(dilauryl phosphite)]; the filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; the average length of the long carbon nanotubes is 800 μm.

[0033] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 15 parts of styrene and 8 parts of divinylbenzene are dissolved in 60 parts of N,N-dimethylformamide and stirred to mix evenly, 4 parts of nitrile rubber are added and stirred evenly, 0.3 parts of benzoyl peroxide are added and stirred and heated to 90°C for reaction for 12 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N,N-dimethylformamide is removed and then the material is cut, and the modified nitrile rubber is obtained after drying.

[0034] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0035] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 130° C., and then stopping stirring to obtain a premix;

[0036] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 50° C., then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 190° C.

[0037] Comparative Example 1

[0038] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 40 parts of modified nitrile rubber, 20 parts of filler, 15 parts of reinforcing fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; the average length of the long carbon nanotubes is 500 μm.

[0039] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0040] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0041] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0042] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0043] Comparative Example 2

[0044] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 40 parts of ethylene-octene copolymer, 20 parts of filler, 15 parts of reinforcing fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotube in a mass ratio of 4:1; the average length of the long carbon nanotube is 500 μm.

[0045] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0046] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0047] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0048] Comparative Example 3

[0049] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified nitrile rubber, 20 parts of ethylene-octene copolymer, 20 parts of ferroboric acid powder, 15 parts of reinforcing fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; the average length of the long carbon nanotubes is 500 μm.

[0050] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0051] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0052] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0053] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0054] Comparative Example 4

[0055] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified nitrile rubber, 20 parts of ethylene-octene copolymer, 20 parts of molybdenum calcium ore powder, 15 parts of reinforcing fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the reinforcing fiber is a mixture of ceramic fiber and long carbon nanotubes in a mass ratio of 4:1; the average length of the long carbon nanotubes is 500 μm.

[0056] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0057] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0058] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0059] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0060] Comparative Example 5

[0061] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified nitrile rubber, 20 parts of ethylene-octene copolymer, 20 parts of filler, 15 parts of ceramic fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixed mineral powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1.

[0062] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0063] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0064] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0065] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0066] Comparative Example 6

[0067] A high-strength PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified nitrile rubber, 20 parts of ethylene-octene copolymer, 20 parts of filler, 15 parts of long carbon nanotubes, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixed mineral powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:1; the average length of the long carbon nanotubes is 500 μm.

[0068] The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 10 parts of styrene and 6 parts of divinylbenzene are dissolved in 45 parts of N, N-dimethylformamide and stirred to mix evenly, 3 parts of nitrile rubber are added and stirred evenly, 0.2 parts of benzoyl peroxide are added and stirred and the temperature is raised to 85° C. to react for 10 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N, N-dimethylformamide is removed and the material is cut, and the modified nitrile rubber is obtained after drying.

[0069] The preparation method of the high-strength PVC pipe is carried out according to the following steps:

[0070] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0071] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0072] Experimental example:

[0073] Corrosion resistance, acid and alkali resistance: 10% hydrochloric acid, 40% sodium hydroxide and 50% sodium chloride were used to test the samples for corrosion. The results are shown in Table 1:

[0074] Table 1

[0075]

[0076] Impact performance: According to GB / T 1843-2008, the specimens were notched with a 2 mm gap for impact testing; each group of experiments was repeated 3 times to obtain the average value, and SPSS24.0 software was used for statistical analysis. The quantitative data results were used to (mean ± standard deviation) was expressed, and the Kolmogorov-Smirnov test was used for data normality test. For data that met the normal distribution, the mean difference between the two groups was compared using the t test, and the difference was considered statistically significant when P < 0.05. The measurement results are shown in Table 2:

[0077] Table 2

[0078]

[0079]

[0080] Note: * represents P < 0.05 compared with the group in Example 1.

[0081] Tensile properties: tested with a universal testing machine in accordance with GB / T1040-92 and a test temperature of 25°C, with a tensile rate of 50 mm / min; Bending properties: tested with a universal testing machine in accordance with GB / T9341-2000 and a test temperature of 25°C, with a pressure head moving speed of 2 mm / min; each group of experiments was repeated 3 times to take the average value, and SPSS24.0 software was used for statistical analysis. The quantitative data results were used (mean ± standard deviation), the Kolmogorov-Smirnov test was used for data normality test, and the t-test was used to compare the mean differences between the two groups for data that met the normal distribution, with P < 0.05 as the difference being statistically significant. The test results are shown in Table 3:

[0082] Table 3

[0083] Experimental Group Tensile strength MPa Bending strength MPa Example 1 55.8±1.7 82.6±2.6 Example 2 56.2±2.1 81.2±2.5 Example 3 54.7±1.8 82.4±1.7 Comparative Example 5 43.3±2.6* 67.6±2.1* Comparative Example 6 41.8±2.2* 69.2±1.4*

[0084] Note: * represents P < 0.05 compared with the group in Example 1.

[0085] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high-strength PVC pipe, characterized in that: The invention is prepared from the following raw materials in parts by weight: 150-250 parts of polyvinyl chloride resin, 10-30 parts of modified nitrile rubber, 10-30 parts of ethylene-octene copolymer, 15-25 parts of filler, 10-20 parts of reinforcing fiber, 1-3 parts of lubricant, 1-3 parts of plasticizer and 1-4 parts of titanate coupling agent.

2. The high-strength PVC pipe according to claim 1, characterized in that: The preparation method of the modified nitrile rubber is as follows: according to the weight proportions, 5-15 parts of styrene and 3-8 parts of divinylbenzene are dissolved in 30-60 parts of N,N-dimethylformamide and stirred to mix evenly, 1-4 parts of nitrile rubber are added and stirred evenly, 0.1-0.3 parts of benzoyl peroxide are added, stirred and heated to 80-90° C. for reaction for 8-12 hours, after the reaction is completed, the reactants are extruded into strips and then immersed in water, the N,N-dimethylformamide is removed and then the material is cut, and the modified nitrile rubber is obtained after drying.

3. The high-strength PVC pipe according to claim 1, characterized in that: The filler is a mixed ore powder of boron iron ore powder and molybdenum calcium ore powder in a mass ratio of 2:

1.

4. The high-strength PVC pipe according to claim 1, characterized in that: The reinforcing fibers are a mixture of ceramic fibers and long carbon nanotubes in a mass ratio of 4:

1.

5. The high-strength PVC pipe according to claim 4, characterized in that: The average length of the long carbon nanotubes is 200-1000 μm.

6. The high-strength PVC pipe according to claim 1, characterized in that: The lubricant is one or more of microcrystalline wax, stearic acid, polypropylene wax and polyethylene wax.

7. The high-strength PVC pipe according to claim 1, characterized in that: The plasticizer is one or more of di(2-ethylhexyl)phthalate, hydrogenated rosin, diisononyl phthalate, and diisodecyl phthalate.

8. The high-strength PVC pipe according to claim 1, characterized in that: The titanate coupling agent is one or more of tris(dioctylpyrophosphoryloxy)titanate isopropyl ester, tetraoctyloxytitanium [di(tridecyl phosphite)], and tetraoctyloxytitanium [di(dilauryl phosphite)].

9. The method for preparing the high-strength PVC pipe according to claim 1, characterized in that: Follow these steps: (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110-130° C., and stopping stirring to obtain a premix; (2) The premix is ​​conveyed to a cold mixer for stirring and cooling to 35-50°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding.

10. The method for preparing the high-strength PVC pipe according to claim 9, characterized in that: The processing temperature of the twin-screw extruder is 170-190°C.

Citation Information

Cited By

  • High-strength corrugated pipe for drainage and manufacturing method thereof

    CN121362410A