Polyphenyl ether modified SEBS hard insulating material with hydrophobic performance

By blending and injection molding with SEBS with polypropylene, modified polyphenylene ether, combined with compounds such as dibenzyltoluene and hydrogenated terphenyl, the deficiency of SEBS-based insulating materials in hydrophobic properties and mechanical strength is solved, and high rigidity is achieved. Insulating materials with long-term hydrophobic and flame retardant properties, suitable for outdoor applications.

CN118978784APending Publication Date: 2024-11-19江苏华厦电力成套设备有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411155079.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing SEBS-based insulating materials are difficult to maintain long-term effects when improving hydrophobic properties, and the processing performance and mechanical strength are insufficient, which cannot meet the requirements of outdoor hard insulating materials.

Method used

Modified polyphenylene by blending hydrogenated styrene-butadiene-styrene block copolymer (SEBS) with polypropylene, modified polyphenylene ether, silicone oil, flame retardant, antioxidant and light stabilizer, using modified polyphenylene Ethers improve the rigidity and hydrophobic properties of the material, and reduce the processing temperature and improve the hydrophobic mobility of the material surface by compounds such as dibenzyltoluene and hydrogenated terphenyl.

Benefits of technology

The long-term hydrophobic, mechanical strength, rigidity and low temperature resistance of SEBS materials have been achieved, the hardness of the material is improved, and the water repellent mobility and flame retardancy are significantly enhanced. It is suitable for outdoor hard insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004722050000041
    Figure BDA0005004722050000041
Patent Text Reader

Abstract

The invention relates to a polyphenyl ether modified SEBS (styrene-butadiene-styrene) hard insulating material with hydrophobic performance, which is prepared by blending and injection molding the following components in parts by weight: 70-100 parts of hydrogenated styrene-butadiene-styrene block copolymer (SEBS), 30-60 parts of polypropylene, 5-30 parts of modified polyphenyl ether, 0.5-5 parts of silicone oil, 40-90 parts of flame retardant, 0.2-1 part of antioxidant and 0.2-1 part of light stabilizer, the modified polyphenyl ether is prepared from 60 to 90 parts by weight of poly (2, 6-dimethyl-1, 4-phenyl ether), 10 to 30 parts by weight of polystyrene, 0.5 to 20 parts by weight of dibenzyl toluene, 0.5 to 20 parts by weight of hydrogenated terphenyl, 5 to 20 parts by weight of silicone and the like, and the polystyrene is polystyrene with high impact resistance; wherein the silicone is a copolymer of polysiloxane and polystyrene. The polyphenyl ether modified SEBS hard insulating material with hydrophobic property has the properties of toughness, insulation, low temperature resistance, hydrophobicity, flame retardance and the like, the Shore D hardness of the material is 50-60, the tensile strength and elongation at break at 23 DEG C are respectively greater than 20 MPa and 400%, the volume resistivity is greater than 1 * 10 < 14 > omega.m, and the surface static water contact angle is greater than 110 degrees.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating materials, and in particular relates to a polyphenylene ether modified SEBS hard insulating material with hydrophobicity. Background Art

[0002] Hydrogenated styrene-butadiene-styrene block copolymer (SEBS for short) is a commonly used thermoplastic elastomer. Since the carbon-carbon double bonds of its butadiene chain segments are hydrogenated and saturated, it exhibits excellent weather resistance, low temperature resistance, and mechanical strength. At present, SEBS has been widely used in the fields of daily necessities, medical equipment, and insulating products. In the field of insulating materials, SEBS is often blended with other polyolefin materials as an insulating resin matrix. For example, the invention patent application CN1 12940437A discloses a crack-resistant flame-retardant wire material and its preparation method, including 10-40 parts of hydrogenated styrene-butadiene block copolymer, 3-15 parts of polyphenylene ether resin, 5-30 parts of polyolefin resin, 10-40 parts of softening oil, etc., to improve the crack resistance of the wire material in an extreme temperature change environment. Invention patent application CN107556688A discloses a halogen-free, scratch-resistant, wear-resistant, and fire-resistant wire insulation material, including 15-25% hydrogenated styrene-butadiene block copolymer, 5-15% mineral oil, 5-15% polypropylene, and 15-25% polyphenylene ether. In the above technology, the compatibility and processing properties of materials such as SEBS and polyphenylene ether are improved by adding a large amount of softening oil / mineral oil. In addition, in order to improve the hydrophobicity of SEBS insulating materials, various silicone oils (or polysiloxanes) can be added. For example, invention patent application CN107001765A discloses an electrical insulating material and a method for preparing an electrical insulating element. The electrical insulating material includes a matrix component, a filler component, and a liquid hydrophobic component, wherein the matrix component includes a saturated styrene block copolymer, and the liquid hydrophobic component includes a liquid fluorinated or chlorinated hydrocarbon, and a cyclic, linear, or branched liquid organic polysiloxane. Invention patent application CN117198659A discloses a hard rubber-plastic composite insulator and preparation method, wherein the shed and sheath materials are blended and injection molded by 80-100 parts of hydrogenated styrene-butadiene-styrene block copolymer, 1-15 parts of methylphenyl silicone oil, 30-50 parts of homopolypropylene, 10-20 parts of copolymer polypropylene, 1-15 parts of maleic anhydride grafted polypropylene, 30-90 parts of flame retardant, etc., and methylphenyl silicone oil is used as a hydrophobic migration agent to improve the hydrophobicity of the material surface. In the above-mentioned technologies, the hydrophobicity of SEBS composite materials is basically improved by adding various silicone oils.

[0003] For outdoor insulation equipment such as insulating bushings and transmission line insulators, it is expected to provide an insulating material with good mechanical strength, rigidity, long-term water repellency, low temperature resistance and other properties. However, the existing SEBS-based insulating material technology is difficult to fully meet these requirements. In the prior art, some adopt the addition of high amounts of softening oil to improve the processing technology of SEBS and its compatibility with materials such as polyphenylene ether, but this will reduce the rigidity (hardness) and mechanical strength of the material; some improve the water repellency of SEBS by adding hydrophobic components such as silicone oil, but silicone oil has poor compatibility with SEBS and is easy to migrate out, which makes it difficult to maintain the water repellency of the material for a long time. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and invent a polyphenylene ether modified SEBS hard insulating material with hydrophobic properties, which also has excellent mechanical strength, rigidity, long-term hydrophobicity, low temperature resistance, flame retardancy and insulation properties and can be used as an outdoor hard insulating material.

[0005] The solution provided by the present invention is: a polyphenylene ether modified SEBS hard insulating material with hydrophobic performance, which is blended and injection-molded by the following components in parts by weight: 70-100 parts of hydrogenated styrene-butadiene-styrene block copolymer (SEBS), 30-60 parts of polypropylene, 5-30 parts of modified polyphenylene ether, 0.5-5 parts of silicone oil, 40-90 parts of flame retardant, 0.2-1 parts of antioxidant and 0.2-1 parts of light stabilizer.

[0006] The modified polyphenylene ether is prepared from 60-90 parts of poly-2,6-dimethyl-1,4-phenylene ether (hereinafter referred to as polyphenylene ether), 10-30 parts of polystyrene, 0.5-20 parts of dibenzyltoluene, 0.5-20 parts of hydrogenated terphenyl and 5-20 parts of silicone, in parts by weight, wherein the polystyrene is preferably high-impact polystyrene; the silicone is a copolymer of polysiloxane and polyolefin, preferably a copolymer of polysiloxane and polystyrene.

[0007] The polystyrene content of the SEBS is 30-35%, where the styrene content refers to the molar content of styrene in the preparation of SEBS.

[0008] The polypropylene has high fluidity, and its melt index is above 30 g / 10 min (230° C., 2.16 kg).

[0009] The flame retardant is composed of a mixture of two or more flame retardants such as decabromodiphenylethane, antimony trioxide, aluminum hydroxide, diethylaluminum hypophosphite, zinc oxide, melamine cyanurate and melamine polyphosphate. The amount of the flame retardant is adjusted according to the flame retardant grade requirements of different insulation equipment.

[0010] The antioxidant is composed of a mixture of antioxidant 1010, antioxidant 168 and antioxidant DLTP.

[0011] The light stabilizer is one or a mixture of two ultraviolet absorbers UV329 and UV531.

[0012] Principle of the invention: SEBS material is an elastomer with excellent low temperature resistance, aging resistance, high elasticity and mechanical strength, but its processing performance is poor and its hardness is not high, so it cannot be used alone as a hard insulating material. The present invention uses polypropylene to improve its processing performance, especially uses modified polyphenylene ether to improve the rigidity, hydrophobicity and flame retardancy of SEBS materials. Polyphenylene ether has excellent mechanical strength, stress relaxation resistance, creep resistance, water resistance, heat resistance, flame retardancy, insulation and other properties, but polyphenylene ether has a high melting point and poor melt fluidity. The molding temperature is generally as high as 280-300°C, and it is difficult to directly blend and granulate with SEBS and PP materials (melt extrusion processing temperature is generally 200-240°C). The present invention uses a certain amount of polystyrene, silicone, hydrogenated terphenyl and dibenzyltoluene to modify polyphenylene ether, and the main effects are as follows: (1) The use of silicone, hydrogenated terphenyl, dibenzyltoluene and polystyrene improves the processing performance of polyphenylene ether and reduces its processing temperature, which can adapt to the processing technology and processing temperature of SEBS and PP. (2) Further research found that compounds such as dibenzyltoluene and hydrogenated terphenyl can not only improve the processing performance of polyphenylene ether, but also have the function of slowly migrating the dirt layer to the surface of the material, that is, making the dirt layer attached to the surface of the insulating material hydrophobic, acting as a hydrophobic migration agent; when used together with the silicone oil component in the formula in a certain proportion, the initial hydrophobic effect is obvious due to the faster migration speed of the silicone oil; dibenzyltoluene and other compounds have good compatibility with SEBS, a slower migration speed, and a long-term hydrophobic effect. The combination of the two can maintain the hydrophobicity of the material surface for a long time, as well as the hydrophobic migration effect to the dirt layer on its surface. (3) Under the volume-enhancing effect of materials such as polystyrene, hydrogenated terphenyl, dibenzyltoluene and silicone, the brittle fracture surface of the modified SEBS material was observed by scanning electron microscopy. It was found that polyphenylene ether was dispersed in SEBS in an aggregated state of several microns to tens of microns, which not only improved the synergistic flame retardant effect of polyphenylene ether, but also prevented the burning and dripping of SEBS. At the same time, the micron-level dispersion of polyphenylene ether did not affect the low-temperature resistance of the modified SEBS composite material, and the low-temperature loss peak temperature measured by its dynamic mechanical properties did not change.

[0013] The preparation method of the modified polyphenylene ether comprises the following steps: putting polyphenylene ether, polystyrene, dibenzyltoluene, hydrogenated terphenyl and silicone into a high-speed mixer in proportion and mixing for 10-20 minutes, and then melting and mixing in an extruder to granulate the modified polyphenylene ether.

[0014] The present invention also provides a method for preparing a polyphenylene ether modified SEBS hard insulating material with hydrophobic properties, comprising the following steps: putting SEBS, polypropylene, modified polyphenylene ether, silicone, flame retardant, antioxidant, light stabilizer, etc. into a high-speed mixer in proportion, the speed of the high-speed mixer is 400-700 rpm, mixing at room temperature for 10-20 minutes to obtain a modified SEBS mixture; adding the obtained modified SEBS mixture into a twin-screw extruder to melt and mix the materials, the temperature is 200-240°C, and the screw speed is 50-200 rpm to obtain a modified SEBS hard insulating material.

[0015] Beneficial effects of the invention: A polyphenylene ether modified SEBS hard insulating material with hydrophobic properties, which has the properties of toughness, insulation, low temperature resistance, long-term hydrophobicity, etc. The Shore D hardness of the material is 50-60, the tensile strength and elongation at break at 23°C are greater than 20MPa and 400% respectively, and the volume resistivity is greater than 1×10 14 Ω·m, and the static water contact angle on the surface is greater than 110°. DETAILED DESCRIPTION

[0016] Example 1

[0017] A polyphenylene ether modified SEBS hard insulating material with hydrophobicity is prepared by blending and injection molding the following components in parts by weight: 80 parts of hydrogenated styrene-butadiene-styrene block copolymer, 40 parts of polypropylene, 15 parts of modified polyphenylene ether, 1 part of silicone oil, 48 parts of flame retardant, 0.6 parts of antioxidant and 0.6 parts of light stabilizer.

[0018] The modified polyphenylene ether is composed of 60 parts of polyphenylene ether, 22 parts of polystyrene, 4 parts of dibenzyltoluene, 4 parts of hydrogenated terphenyl and 10 parts of silicone, in parts by weight, wherein the silicone is a copolymer of polysiloxane and impact-resistant polystyrene.

[0019] Example 2

[0020] A polyphenylene ether modified SEBS rigid insulating material with hydrophobicity is prepared by blending and injection molding the following components in parts by weight: 70 parts of hydrogenated styrene-butadiene-styrene block copolymer, 50 parts of polypropylene, 15 parts of modified polyphenylene ether, 1 part of silicone oil, 48 parts of flame retardant, 0.6 parts of antioxidant and 0.6 parts of light stabilizer.

[0021] The modified polyphenylene ether is composed of 60 parts of polyphenylene ether, 24 parts of polystyrene, 7.5 parts of dibenzyltoluene, 0.5 parts of hydrogenated terphenyl and 8 parts of silicone, in parts by weight, wherein the silicone is a copolymer of polysiloxane and impact-resistant polystyrene.

[0022] Comparative Example

[0023] A SEBS insulating material is formed by blending and injection molding the following components in parts by weight: 80 parts of hydrogenated styrene-butadiene-styrene block copolymer, 40 parts of polypropylene, 1 part of silicone oil, 48 parts of flame retardant, 0.6 parts of antioxidant and 0.6 parts of light stabilizer.

[0024] The difference between the comparative example and Example 1 is that no modified polyphenylene ether is added.

[0025] The main properties of the materials of the examples and comparative examples are shown in Table 1, where the hydrophobicity grade HC of the sample contaminated surface is 0.6 mg / cm after the sample surface is contaminated (the salt density + ash density of the standard contamination layer is 0.6 mg / cm 2 ) 96h test: Use the spray method to spray 10-20mL of deionized water on the sample surface within 20s. Determine the wettability according to GB / T 24622-2009 and judge the hydrophobicity of the sample surface. The hydrophobicity level is divided into 7 levels: HC1-HC7, HC1 means the most hydrophobic and HC7 means the most hydrophilic.

[0026] Table 1 Comparison of main properties of examples and comparative examples

[0027]

[0028]

[0029] It can be seen from Table 1 that compared with the main properties of the comparative example, the material of the embodiment has higher hydrophobic migration (the hydrophobicity grade of the contaminated surface is HC2), rigidity (Shore D hardness higher than 50°) and flame retardancy (V0 grade, no dripping) while maintaining the excellent tensile strength, elongation at break, insulation and low temperature resistance of the material.

Claims

1. A polyphenylene ether modified SEBS rigid insulating material with hydrophobic properties, which is formed by blending and injection molding the following components: 70-100 parts of hydrogenated styrene-butadiene-styrene block copolymer SEBS, 30-60 parts of polypropylene, 0.5-5 parts of silicone oil, 40-90 parts of flame retardant, 0.2-1 parts of antioxidant and 0.2-1 parts of light stabilizer, characterized in that There are also 5 to 30 parts of modified polyphenylene ether; the modified polyphenylene ether is prepared by weight from 60 to 90 parts of poly 2,6-dimethyl-1,4-phenylene ether, 10 to 30 parts of polystyrene, 0.5 to 20 parts of dibenzyltoluene, 0.5 to 20 parts of hydrogenated terphenyl and 5 to 20 parts of silicone, wherein the polystyrene is high-impact polystyrene; and the silicone is a copolymer of polysiloxane and polystyrene.

Citation Information

Patent Citations

  • Electrical insulating material and method for preparing insulating material element

    CN107001765A

  • Halogen-free, anti-scratch, anti-abrasion and fireproof electric wire insulation material

    CN107556688A

  • Anti-cracking flame-retardant wire material and preparation method thereof

    CN112940437A

  • Hard rubber and plastic composite insulator and preparation method thereof

    CN117198659A