Preparation method and application of non-noble metal catalyst

By preparing cobalt-based catalysts on the support precipitation method and performing pre-reduction treatment, the problems of low activity and insufficient production efficiency of non-precious metal catalysts are solved, and the efficiency and selectivity of the hydrogenation reaction of organic liquids are significantly improved, and efficient hydrogen storage is achieved performance.

CN119056451APending Publication Date: 2024-12-03CHINA HYDROGEN YUANAN (SHANGHAI) HYDROGEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411268609.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing organic liquid hydrogen storage technology, the catalytic activity of non-precious metal catalysts is low and the production process efficiency is not high, which limits their promotion in large-scale applications, especially in the hydrogenation reaction, with insufficient product selectivity and stability.

Method used

By using cobalt as an active component and loading it on support such as Al2O3, SiO2, TiO2, etc., the catalyst is prepared by precipitation method, controlling the temperature, pH value and aging time during the precipitation process, and combining washing, drying and calcining steps, an ideal preparation is prepared It is a non-precious metal catalyst with performance and is subjected to pre-reduction treatment before use, and is suitable for hydrogenation reaction of unsaturated organic liquids.

Benefits of technology

The catalyst is achieved with high activity and stability, and the efficiency and selectivity of the hydrogenation reaction of organic liquids are improved. Especially in the hydrogenation process of benzyl toluene and dibenzyl toluene, the hydrogenation degree of the catalyst reaches 90% and 82% %, significantly improving hydrogen storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention is applicable to the technical field of organic liquid hydrogen storage, and provides a preparation method of a non-noble metal catalyst, which comprises the following steps: mixing a proper amount of active metal salt with deionized water to obtain an active metal salt solution; mixing a proper amount of alkali with deionized water to obtain a precipitation solution; dispersing a proper amount of a carrier in deionized water and continuously stirring to form a uniformly mixed carrier suspension; dropwise adding the active metal salt solution and the precipitation solution into the carrier suspension at the same time for precipitation to obtain a catalyst precursor suspension; and aging and filtering the catalyst precursor suspension to obtain a catalyst precursor, and washing, drying and calcining the catalyst precursor to obtain the hydrogenation catalyst. The catalyst prepared by the method is specially used for hydrogenation of organic liquid, active metals are uniformly dispersed, and different active metals have a good synergistic effect. When the catalyst is applied to the hydrogenation process of hydrogen storage materials such as benzyl toluene and dibenzyl toluene, excellent hydrogen storage performance can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic liquid hydrogen storage, and in particular relates to a preparation method and application of a non-precious metal catalyst. Background Art

[0002] As a clean and renewable energy source, hydrogen has become an effective choice for meeting future energy challenges due to its high energy density, zero carbon emissions and abundant sources. The concept of "hydrogen economy" was first proposed in the mid-1970s and is now seen as a viable solution to energy and environmental problems. However, the use of hydrogen as an energy carrier still faces major challenges, mainly in two aspects. First, the volume energy density of hydrogen at room temperature and pressure (0.003kWh L -1 ) is low, making storage and transportation inefficient. Secondly, the safety hazards caused by hydrogen's flammability and wide explosion limits hinder its large-scale and efficient storage, requiring specialized infrastructure to deal with these problems. To solve these problems, new and convenient hydrogen storage and transportation methods are urgently needed.

[0003] In recent years, in order to meet the hydrogen storage standards set by the U.S. Department of Energy for mobile applications (5.5wt% and 40g L -1 ), a variety of technologies have been developed, including compressed hydrogen, liquid hydrogen, metal hydrides, and adsorption of hydrogen in porous materials. These state-of-the-art technologies involve storing hydrogen in elemental form or on solid materials using physical or chemical adsorption. A comprehensive overview of these methods has been given in previous reports. Current hydrogen storage technologies mainly include physical hydrogen storage and chemical hydrogen storage. Physical hydrogen storage faces the problems of high equipment requirements and harsh operating conditions, which affect its performance and efficiency. Liquid organic hydride hydrogen storage technology has attracted attention due to its large hydrogen storage capacity, high energy density, and convenient liquid storage and transportation characteristics. This technology stores hydrogen by catalyzing the hydrogenation and reversible dehydrogenation reactions of unsaturated aromatic hydrocarbons with hydrides (such as cycloalkanes). The reaction process is reversible, the reaction products can be recycled, and the hydrogen reserves are relatively high (about 60-75kgH2 / m 3 , mass fraction 6-8%). In addition, this liquid hydrogen storage method also helps to solve the problem of uneven distribution of energy in different regions.

[0004] The hydrogenation and dehydrogenation processes of organic liquids rely on highly active catalysts, especially in reversible hydrogenation and dehydrogenation reactions. In recent years, precious metal catalysts (such as platinum, palladium, and ruthenium) have been widely used in the field of dehydrogenation catalysis for organic liquid hydrogen storage, and have attracted great attention from researchers due to their excellent catalytic activity. However, the high cost of precious metals limits their widespread use in practical applications, which poses a challenge to the large-scale promotion of organic liquid hydrogen storage technology. Therefore, researchers began to explore the use of non-precious metal catalysts (such as nickel, iron, cobalt, etc.) to replace precious metals, aiming to improve the economy and practicality of organic liquid dehydrogenation reactions.

[0005] In recent years, non-precious metal catalysts such as cobalt-based catalysts have been used in organic liquid hydrogenation reactions. Studies have shown that cobalt-based catalysts have low activity in hydrogenation reactions, but the hydrogenation conversion of unsaturated organic liquids can be promoted by increasing the cobalt loading in the catalyst, increasing the reaction temperature or the reaction pressure. However, the selectivity of hydrogenation products of this method is low because hydrogenation and dehydrogenation occur simultaneously in the reaction and there is a competitive relationship.

[0006] Although conventional non-precious metal supported catalysts offer an alternative, they still have inherent problems. First, the catalytic activity of these catalysts is usually not high enough to achieve the desired hydrogenation effect, and the stability of hydrogenation needs to be improved. In addition, the existing production process also has shortcomings and needs to be further optimized to reduce costs and improve efficiency. Summary of the invention

[0007] The purpose of the embodiments of the present invention is to provide a preparation method and application of a non-precious metal catalyst, aiming to solve the problems raised in the above background technology.

[0008] The embodiment of the present invention is implemented as follows: a method for preparing a non-precious metal catalyst, in which cobalt is used as an active component and loaded on a series of carriers such as Al2O3, SiO2, and TiO2.

[0009] The preparation of the catalyst can be achieved by precipitation, wherein the precipitation process involves the reaction of a metal salt and an alkali in a carrier suspension. The metal salt can be selected from one or more of nitrates, acetates, halides or sulfates, wherein nitrates and acetates are preferred, and the concentration range of the metal salt solution is 0.01 to 5 mol / L, and the recommended concentration is 0.1 to 4 mol / L. The alkali in the precipitation reaction can be selected from soluble carbonates (such as sodium carbonate, potassium carbonate), hydroxides (such as sodium hydroxide, potassium hydroxide), ammonium carbonate or ammonia water, and sodium carbonate, ammonium carbonate, sodium hydroxide or ammonia water are recommended. The molar concentration range of the alkali is 0.01 to 5 mol / L, and the preferred range is 0.1 to 4 mol / L. The carrier should be dispersed in deionized water and form a uniform suspension under continuous stirring. The carrier can be one or more of aluminum oxide, magnesium oxide, manganese oxide, silicon oxide or activated carbon, preferably aluminum oxide, magnesium oxide and silicon oxide. The volume ratio of the carrier to the deionized water should be between 0.1:1 and 10:1, and the recommended volume ratio is 1:1 to 10:1. This method can effectively control the structure and performance of the catalyst to meet different application requirements.

[0010] The metal salt solution and the precipitate are simultaneously added dropwise to the carrier suspension for precipitation to form a catalyst precursor suspension. The temperature of the precipitation process should be controlled in the range of -20 to 80°C, preferably between 10 and 80°C; the pH value of the precipitation should be maintained between 6 and 10, preferably between 7 and 10. After the precipitation reaction is completed, the catalyst precursor needs to be aged for 0 to 50 hours, preferably 1 to 30 hours.

[0011] The aged catalyst precursor suspension needs to be filtered to obtain the catalyst precursor. Next, the catalyst precursor needs to be washed, dried and calcined. The standard of the washing process is that the pH value of the last washing liquid should be between 7 and 8, preferably between 7 and 7.5.

[0012] Drying can be carried out under vacuum conditions, air atmosphere or inert atmosphere, preferably air atmosphere or inert atmosphere. The drying temperature ranges from 20 to 200°C, preferably 50 to 150°C, and the drying time is 1 to 100 hours, preferably 10 to 80 hours. The calcination process can also be carried out under vacuum, air or inert atmosphere, preferably air or inert atmosphere. The calcination temperature should be between 200 and 800°C, preferably 300 to 600°C, and the calcination time is 1 to 100 hours, preferably 3 to 50 hours. Through this series of steps, a dehydrogenation catalyst with ideal performance can be obtained.

[0013] Another object of the present invention is to use a non-precious metal catalyst, wherein the prepared non-precious metal catalyst is used in a hydrogenation reaction of an organic liquid, and a pre-reduction treatment is required before the catalyst is used. The reducing atmosphere can be hydrogen or diluted hydrogen. The temperature of the reduction process should be between 200 and 800° C., preferably 300 to 600° C., and the reduction time is 1 to 100 hours, preferably 1 to 50 hours.

[0014] The non-precious metal catalyst is suitable for hydrogenation of unsaturated organic liquids. These organic liquids include benzyltoluene, dibenzyltoluene, toluene, quinoline, carbazole and N-ethylcarbazole. The temperature range of the hydrogenation reaction is 150 to 300°C, preferably 180 to 250°C; the reaction pressure range is 1MPa to 8MPa, preferably 4MPa to 6MPa.

[0015] The present invention provides a method for preparing a non-precious metal catalyst. The catalyst prepared by the method is specifically used for hydrogenation of organic liquids, has uniform dispersion of active metals and good synergistic effects between different active metals. The catalyst is applied to the hydrogenation process of hydrogen storage materials such as benzyltoluene and dibenzyltoluene, and can achieve excellent hydrogen storage performance. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0017] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0018] An embodiment of the present invention provides a method for preparing a non-precious metal catalyst, comprising the following steps:

[0019] Step 1: Mix an appropriate amount of active metal salt with deionized water to obtain an active metal salt solution; mix an appropriate amount of alkali with deionized water to obtain a precipitate; disperse an appropriate amount of carrier in deionized water and continue stirring to form a uniformly mixed carrier suspension;

[0020] Step 2: simultaneously adding the active metal salt solution and the precipitate solution to the carrier suspension for precipitation to obtain a catalyst precursor suspension;

[0021] Step 3: The catalyst precursor suspension is aged and filtered to obtain a catalyst precursor, which is then washed, dried and calcined to obtain a hydrogenation catalyst.

[0022] As a preferred embodiment of the present invention, in step 1, the active metal is cobalt; the active metal salt is one or more of nitrate, acetate, halide and sulfate; the concentration of the active metal salt solution is 0.01-5 mol / L.

[0023] In the embodiment of the present invention, the active metal salt is preferably nitrate and acetate, and the preferred concentration range is 0.1-4 mol / L.

[0024] As a preferred embodiment of the present invention, in step 1, the alkali is one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate, potassium bicarbonate and ammonium bicarbonate; and the molar concentration of the alkali is 0.01 to 5 mol / L.

[0025] In the embodiment of the present invention, the base is preferably sodium carbonate, ammonium carbonate, sodium hydroxide or ammonia water, and the preferred concentration range is 0.1 to 4 mol / L.

[0026] As a preferred embodiment of the present invention, in step 1, the carrier is one or more of aluminum oxide, magnesium oxide, manganese oxide, silicon oxide and activated carbon; the volume ratio of the carrier to the volume of deionized water is 0.1:1 to 10:1.

[0027] In an embodiment of the present invention, the carrier is preferably aluminum oxide, magnesium oxide and silicon oxide; the preferred volume ratio is 1:1 to 10:1.

[0028] As a preferred embodiment of the present invention, in step 2, the pH of the suspension is maintained at 6 to 10, preferably 7 to 10 during the precipitation process; the temperature of the suspension during the precipitation process is -20 to 80°C, preferably between 10 and 80°C.

[0029] As a preferred embodiment of the present invention, in step 3, the aging temperature is -20 to 80°C, the aging time is 0 to 50 hours, and the aging pH is 6 to 10;

[0030] The standard for washing completion is that the pH value of the last washing solution is between 7 and 8, preferably between 7 and 7.5;

[0031] The drying temperature is 20 to 200° C., preferably 50 to 150° C.; the drying time is 1 to 100 hours, preferably 10 to 80 hours;

[0032] The calcination temperature is 200 to 800° C., preferably 300 to 600° C.; the calcination time is 1 to 100 hours, preferably 3 to 50 hours.

[0033] Another embodiment of the present invention provides an application of a non-precious metal catalyst, which is a non-precious metal catalyst prepared based on the above-mentioned preparation method of the non-precious metal catalyst. The non-precious metal catalyst is applied to the hydrogenation reaction of an organic liquid, and the non-precious metal catalyst needs to be reduced before use.

[0034] As a preferred embodiment of the present invention, the organic liquid is one or more of benzyltoluene, dibenzyltoluene, toluene, quinoline, carbazole and N-ethylcarbazole.

[0035] As a preferred embodiment of the present invention, the reducing atmosphere of the catalyst is pure hydrogen; the reducing temperature of the catalyst is 200-800° C., preferably 300-600° C.; the reducing time of the catalyst is 1-100 h, preferably 1-50 h.

[0036] As a preferred embodiment of the present invention, the hydrogenation reaction temperature of the organic liquid is 150-300° C., preferably 180-250° C.; the reaction pressure of the catalyst is 1 MPa-8 MPa, preferably 4 MPa-6 MPa.

[0037] Several specific examples are provided below to verify the effectiveness of this method:

[0038] Example 1: Weigh 13.5 grams of cobalt nitrate hexahydrate, add it to deionized water, stir it evenly at room temperature to make an impregnation solution. At the same time, weigh 13.35 grams of ammonium carbonate and add it to deionized water to form a precipitate. The above two liquids are simultaneously added dropwise to deionized water containing 6 grams of aluminum oxide, and continue to stir at room temperature for 4 hours. Subsequently, wash and dry the sample at 80°C. After the dried catalyst is fully ground, it is calcined at 450°C for 6 hours. The obtained catalyst is the calcined catalyst (Co / Al2O3). After the calcined catalyst is ground, it is pressed into tablets and sieved into 40-60 mesh particles. Take an appropriate amount of 40-60 mesh catalyst and quartz sand in a ratio of 1:1, mix and dilute, and then evaluate in a trickle bed apparatus. The reduction process adopts the following heating program: heat from room temperature to 120°C within 30 minutes and keep it for 60 minutes; then heat to 450°C at a heating rate of 1°C / min and keep it for 5 hours. After the reduction is completed, the temperature is lowered to 250°C and maintained for 10 minutes, and the reaction pressure is increased to 5 MPa and maintained. Then the metering pump is turned on to start sampling, the tail gas is analyzed by chromatography, and the hydrogenation liquid is qualitatively and quantitatively analyzed by GC-MS.

[0039] Example 2: Weigh 13.5g of cobalt nitrate trihydrate and add it to deionized water and stir it evenly at room temperature to prepare an impregnation solution. Weigh 13.35g of ammonium carbonate and add it to deionized water to form a precipitate. Both are added dropwise to deionized water added with 6g of silicon oxide and stirred at room temperature for 4h. Then wash and dry the sample at 80°C. The dried catalyst is fully ground and calcined at 450°C for 6h. The resulting catalyst is the calcined catalyst (Co / SiO2). The calcined catalyst is pressed and sieved into 40-60 mesh particles after grinding. Weigh an appropriate amount of 40-60 mesh catalyst and dilute it with quartz sand in a ratio of 1:1, and evaluate it in a trickle bed device. The reduction heating program is: 30min from room temperature to 120°C, then keep it for 60min; then heat it to 450°C at a heating rate of 1°C / min and keep it for 5h. After the reduction is completed, cool it to 250°C and keep it for 10min, and increase the reaction pressure to 5MPa and keep it. Then the metering pump was turned on to start sampling, the tail gas was analyzed by chromatography, and the hydrogenated liquid was qualitatively and quantitatively analyzed by GC-MS.

[0040] Example 3: Dissolve 13.5 grams of cobalt nitrate hexahydrate in deionized water and stir until completely dissolved to prepare an impregnation solution. At the same time, dissolve 13.35 grams of ammonium carbonate in deionized water to form a precipitate. Add the two liquids simultaneously dropwise into deionized water containing 6 grams of titanium oxide and stir at room temperature for 4 hours. Subsequently, the mixed sample is washed and dried at 80°C. The dried catalyst is fully ground and then calcined at 450°C for 6 hours to obtain a calcined catalyst (Co / TiO2). The calcined catalyst is then ground, tableted and sieved into 40-60 mesh particles. Take an appropriate amount of 40-60 mesh catalyst and mix and dilute it with quartz sand in a 1:1 ratio, and evaluate the catalytic performance in a trickle bed apparatus. The reduction process was carried out according to the following temperature program: the temperature was raised from room temperature to 120°C within 30 minutes and maintained for 60 minutes, then raised to 450°C at a heating rate of 1°C / min and maintained for 5 hours, and finally cooled to 250°C and maintained for 10 minutes, and the reaction pressure was increased to 5 MPa and maintained. The metering pump was started for sampling, the tail gas was analyzed by chromatography, and the hydrogenated liquid was qualitatively and quantitatively analyzed by GC-MS.

[0041] Example 4: 6.75 grams of nickel nitrate hexahydrate and 6.75 grams of cobalt nitrate hexahydrate are dissolved in deionized water and stirred evenly at room temperature to obtain an impregnation solution. At the same time, 13.35 grams of sodium carbonate are dissolved in deionized water to form a precipitate. The two liquids are simultaneously added dropwise to deionized water containing 6 grams of aluminum oxide and stirred at room temperature for 4 hours. Thereafter, the sample is washed and dried at 80°C. After the dried catalyst is fully ground, it is calcined at 450°C for 6 hours to obtain a calcined catalyst (NiCo / Al2O3). The calcined catalyst is ground again, pressed into tablets and sieved into 40-60 mesh particles. Take an appropriate amount of 40-60 mesh catalyst and mix and dilute it with quartz sand in a 1:1 ratio, and then evaluate the catalytic performance in a trickle bed apparatus. The temperature program of the reduction process was as follows: the temperature was raised from room temperature to 120 °C within 30 min and maintained for 60 min, then raised to the reduction temperature at a heating rate of 1 °C / min and maintained for 5 h, and finally cooled to 25 0℃ and maintain, increase the reaction pressure to 5MPa and maintain. Start the metering pump for sampling, the tail gas is analyzed by chromatography, and the hydrogenated liquid is analyzed qualitatively and quantitatively by GC-MS.

[0042] Example 5: Dissolve 6.75 grams of copper nitrate trihydrate and 6.75 grams of cobalt nitrate hexahydrate in deionized water, stir evenly at room temperature to obtain an impregnation solution. At the same time, dissolve 13.35 grams of ammonium carbonate in deionized water to form a precipitate. Add the two liquids simultaneously to deionized water containing 6 grams of silicon oxide and stir at room temperature for 4 hours. Wash the sample and dry it at 80°C. The dried catalyst is fully ground and then calcined at 450°C for 6 hours to obtain a calcined catalyst (NiCo / SiO2). The calcined catalyst is ground again, pressed into tablets and sieved into 40-60 mesh particles. After mixing and diluting an appropriate amount of 40-60 mesh catalyst with quartz sand in a 1:1 ratio, it is evaluated in a trickle bed apparatus. The temperature program of the reduction process is: heating from room temperature to 120°C within 30 minutes and maintaining for 60 minutes, then heating to 450°C at a heating rate of 1°C / min and maintaining for 5 hours, finally cooling to 250°C and maintaining for 10 minutes, and increasing the reaction pressure to 5MPa and maintaining. The metering pump is started for sampling, the tail gas is analyzed by chromatography, and the hydrogenated liquid is qualitatively and quantitatively analyzed by GC-MS.

[0043] The hydrogenation capacity of each embodiment is shown in Table 1 below:

[0044] Table 1 Catalyst hydrogenation capacity for benzyltoluene and dibenzyltoluene organic liquids

[0045]

[0046] From the above results, it can be seen that the non-precious metal catalyst prepared by the method of the present invention exhibits a high dehydrogenation efficiency in the hydrogenation reaction of organic matter. In particular, in the hydrogenation reaction of organic hydrogen storage materials, the catalyst has a hydrogenation degree of 90% for benzyltoluene and a hydrogenation degree of 82% for dibenzyltoluene.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a non-precious metal catalyst, characterized in that: The following steps are involved: Step 1: Mixing an active metal salt with deionized water to obtain an active metal salt solution; mixing an alkali with deionized water to obtain a precipitate; dispersing a carrier in the deionized water and continuously stirring to form a uniformly mixed carrier suspension; Step 2: simultaneously adding the active metal salt solution and the precipitate solution to the carrier suspension for precipitation to obtain a catalyst precursor suspension; Step 3: The catalyst precursor suspension is aged and filtered to obtain a catalyst precursor, which is then washed, dried and calcined to obtain a hydrogenation catalyst.

2. The method for preparing a non-precious metal catalyst according to claim 1, characterized in that: In the step 1, the active metal is cobalt; The active metal salt is one or more of nitrate, acetate, halide and sulfate; The concentration of the active metal salt solution is 0.01-5 mol / L.

3. The method for preparing a non-precious metal catalyst according to claim 1, characterized in that: In step 1, the base is one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate, potassium bicarbonate and ammonium bicarbonate; The molar concentration of the base is 0.01 to 5 mol / L.

4. The method for preparing a non-precious metal catalyst according to claim 1, characterized in that: In step 1, the carrier is one or more of aluminum oxide, titanium oxide, manganese oxide, silicon oxide and activated carbon; The volume ratio of the carrier to the deionized water is 0.1:1 to 10:

1.

5. The method for preparing a non-precious metal catalyst according to claim 1, characterized in that: In step 2, the pH of the suspension is maintained at 6 to 10 during the precipitation process; The suspension temperature during the precipitation process is -20 to 80°C.

6. The method for preparing a non-precious metal catalyst according to claim 1, characterized in that: In step 3, the aging temperature is -20 to 80°C, the aging time is 0 to 50 hours, and the aging pH is 6 to 10; The standard for washing completion is that the pH value of the last washing solution is between 7 and 8; The drying temperature is 20 to 200°C; the drying time is 1 to 100 hours; The calcination temperature is 200-800°C; the calcination time is 1-100h.

7. An application of a non-precious metal catalyst, a non-precious metal catalyst prepared by the method for preparing a non-precious metal catalyst according to any one of claims 1 to 6, characterized in that: The non-precious metal catalyst is applied to the hydrogenation reaction of organic liquid, and the non-precious metal catalyst needs to be reduced before use.

8. The use of the non-precious metal catalyst according to claim 7, characterized in that: The organic liquid is one or more of benzyltoluene, dibenzyltoluene, toluene, quinoline, carbazole and N-ethylcarbazole.

9. The use of the non-precious metal catalyst according to claim 8, characterized in that: The reducing atmosphere of the catalyst is pure hydrogen; The reduction temperature of the catalyst is 200 to 800°C; The reduction time of the catalyst is 1 to 100 hours.

10. The use of the non-precious metal catalyst according to claim 9, characterized in that: The hydrogenation reaction temperature of the organic liquid is 150-300°C; The reaction pressure of the catalyst is 1 MPa to 8 MPa.