Porous reduced graphene oxide aerogel / resin wave-absorbing material and preparation method thereof

By introducing porous structures and resin coating into graphene oxide aerogel, the problems of unstable dielectric properties and large thickness of existing electromagnetic wave absorbing materials are solved, and porous reduced graphite oxide with thin thickness and stable dielectric properties are achieved An olefin aerogel/resin absorbing material has wide temperature domain absorbing performance and low dielectric temperature dependence.

CN118978787AActive Publication Date: 2024-11-19NORTHWESTERN POLYTECHNICAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411279032.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

Existing medium/high temperature electromagnetic wave absorbing materials have problems such as obvious dielectric performance fluctuations with temperature, large thickness, poor impedance matching performance, and high conductivity loss, which is difficult to meet the demanding needs of future aircraft.

Method used

The preparation method of porous reduced graphene oxide aerogel/resin absorbing material is adopted, and the nano/micrometer-level pore structure is formed by using ferric nitrate nitrate nitrate as a pore-making agent, combined with freeze-drying and resin impregnation technology, and the resin coats the graphene sheet. The layer is adjusted to adjust the pH value and heat treatment conditions, control the iron-carbon solution reaction, and form a graded pore structure to improve impedance matching and wide temperature domain absorption performance.

Benefits of technology

A porous reduced graphene oxide aerogel/resin absorbing material with thin thickness, stable dielectric properties and excellent wide temperature domain absorption performance, with an effective absorption bandwidth of 4.2GHz, covering the X-band, and the reflection loss value reaches -41.6dB , meets the performance requirements of "thin, wide, light, strong" and low dielectric temperature dependence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978787A_ABST
    Figure CN118978787A_ABST
Patent Text Reader

Abstract

The invention discloses a porous reduced graphene oxide aerogel / resin wave-absorbing material and a preparation method thereof, and belongs to a resin-based wave-absorbing material. The method comprises the following steps: placing iron nitrate nonahydrate in graphene oxide, and forming a graphene oxide uniform dispersion based on electrostatic stability by regulating solution potential; carrying out iron-carbon solid solution at high temperature to generate Fe3C, and carrying out heat treatment on the graphene oxide to generate reduced graphene oxide; after Fe3C is removed through etching, nanoscale holes are formed in the reduced graphene oxide; the generated graphene oxide with holes is wrapped by resin, and part of nano-scale holes are converted into micron-scale holes under the action of the resin; and finally, the reduced graphene oxide aerogel / resin wave-absorbing material comprising graded pores is formed. The nano-pores can enhance the polarization relaxation capability of the material, and the micron-pore structure can improve the impedance matching characteristic of the material, trigger multiple reflection of electromagnetic waves and prolong the propagation path of the electromagnetic waves in the material, thereby enhancing the loss of the electromagnetic waves.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resin-based absorbing materials, and specifically relates to a porous reduced graphene oxide aerogel / resin absorbing material and a preparation method thereof. Background Art

[0002] With the improvement of the coordinated strike capability of multi-site radar network detection and interception systems, stealth performance has become the key to the survival and penetration of future aircraft on the battlefield. Electromagnetic absorbing materials are an important way to achieve aircraft radar stealth. Most of the existing electromagnetic absorbing materials used in medium / high temperatures are dielectric lossy materials. There are problems such as obvious fluctuations in dielectric properties with temperature and large material thickness required to achieve effective electromagnetic absorption, which greatly limits their engineering applications. Therefore, it is of great significance to study electromagnetic absorbing materials with thin thickness and dielectric properties that are insensitive to temperature changes.

[0003] Compared with high-density magnetic materials and semiconductor ceramic materials, carbon materials have the advantages of low density, high chemical stability, and low preparation cost. They are currently the most widely studied absorbing material system. Among them, graphene can achieve better electromagnetic absorbing performance at a lower filling amount due to its unique two-dimensional planar structure, low density, high specific surface area, and excellent carrier mobility, making it one of the important candidates for the development of high-performance absorbing materials. When facing more demanding service environments in the future, graphene has problems such as poor impedance matching, strong conductivity loss characteristics, insufficient dielectric stability over a wide temperature range, and narrow effective absorption bandwidth (reflection loss RL <10dB), which makes it difficult to meet the needs of engineering applications. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a porous reduced graphene oxide aerogel / resin absorbing material and a preparation method thereof. The method combines freeze drying with resin impregnation process to prepare a wide temperature range absorbing composite material, thereby solving the problems of poor impedance matching performance, high conductivity loss and strong dielectric temperature dependence.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a porous reduced graphene oxide aerogel / resin absorbing material comprises the following steps:

[0007] Step 1, placing graphene oxide slurry in deionized water, and obtaining a graphene oxide aqueous solution by magnetic stirring;

[0008] Step 2: Place ferric nitrate nonahydrate in a graphene oxide aqueous solution, mix well, add ammonia water to adjust the pH value of the solution, and freeze-dry to obtain a loaded Fe 3+ Graphene oxide aerogel;

[0009] Step 3: Load Fe 3+ After heat treatment of graphene oxide aerogel, Fe 3 C reduced graphene oxide aerogel, loaded with Fe 3 The reduced graphene oxide aerogel of C is soaked in hydrochloric acid and dried to obtain a porous reduced graphene oxide aerogel;

[0010] Step 4, placing the porous reduced graphene oxide aerogel in a resin solution, impregnating it at normal pressure, and then curing it to obtain a porous reduced graphene oxide aerogel / resin absorbing material.

[0011] A further improvement of the present invention is:

[0012] Preferably, in step 1, the concentration of the graphene oxide aqueous solution is 3 to 5 mg / mL.

[0013] Preferably, in step 2, the mass ratio of the ferric nitrate nonahydrate to the graphene oxide in the graphene oxide aqueous solution is 0.1 to 0.3.

[0014] Preferably, in step 2, the pH value of the solution is adjusted to 7-10.

[0015] Preferably, in step 3, the heat treatment temperature is 900-1200° C., and the heat treatment time is 1-3 hours.

[0016] Preferably, in step 3, the concentration of hydrochloric acid is 10-30wt.%, the soaking time is 24h, the drying temperature is 80°C, and the drying time is 2h.

[0017] Preferably, in step 4, the solvent of the resin solution is anhydrous ethanol, and the concentration of the resin solution is 0.1 to 0.3 g / mL.

[0018] Preferably, in step 4, the normal pressure impregnation time is 0.5 to 1 h.

[0019] Preferably, in step 4, the curing temperature is 160° C. and the curing time is 1 hour.

[0020] A porous reduced oxide graphene aerogel / resin absorbing material prepared by any one of the above preparation methods comprises a graphene sheet layer, wherein the graphene sheet layer is coated with resin and has nano-scale pores and micro-scale pores distributed on the graphene sheet layer.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention discloses a method for preparing a porous reduced graphene oxide aerogel / resin wave absorbing material. In the method, ferric nitrate nonahydrate is placed in graphene oxide, and ferric nitrate nonahydrate is used as a pore-forming agent. Fe metal has high catalytic decomposition activity of carbon precursor, moderate carbon dissolving capacity, and moderate carbon bonding capacity. At the same time, ferric nitrate exhibits strong oxidizing property to oxygen-containing functional groups, and reacts with oxygen-containing functional groups such as hydroxyl and carbonyl in graphene oxide, thereby removing oxygen atoms, and forming Fe-carbon solid solution at high temperature. 3 C, Fe is removed by hydrochloric acid etching 3 After C, the corresponding holes can be formed.

[0023] During the preparation process, the method adjusts the metal cation adsorption efficiency and Zeta potential by controlling the pH value of the solution, and forms a uniform graphene dispersion based on electrostatic stabilization. At the same time, under the action of electrostatic attraction, the metal cations preferentially combine with the oxygen-containing functional groups in the graphene oxide, ensuring the uniform dispersion of the metal cations on the graphene sheets.

[0024] This method uses freeze-drying technology to fix the graphene uniform dispersion, avoiding the accumulation of graphene sheets due to van der Waals action during the reduction process; and uses iron-carbon solid solution reaction to etch the graphene sheets. 3 C and then synthesize porous reduced graphene oxide aerogel. In step 3, the pores in the porous graphene oxide aerogel formed are nanoscale. After being impregnated with resin, under the action of the surface tension of the resin solution, the size of the nanoscale pores is increased, and some of the nanoscale pores become micrometer-level, forming a porous reduced graphene oxide aerogel / resin composite material with a hierarchical pore structure, wherein the nano / micrometer-level pores are evenly distributed on the graphene sheet layer, thereby enhancing the wide temperature range wave absorbing performance of the composite material. In addition, the resin, as an insulating phase, coats the reduced graphene oxide sheet layer, destroys the three-dimensional conductive network structure formed by the overlap of the reduced graphene oxide sheet layers, hinders electron transmission, further reduces the conductive performance, and improves impedance matching. After curing, the resin improves the hardness and stability of the entire wave absorbing material. The synergistic effect of the heterogeneous phase and the hierarchical pores increases the interface polarization loss and reduces the conductivity loss, thereby obtaining a wide temperature wave absorbing material with low dielectric temperature dependence.

[0025] Furthermore, the heat treatment process reduces the graphene oxide, and an iron-carbon solid solution reaction can occur simultaneously during the high-temperature heat treatment reduction process, which simplifies the process. The degree of iron-carbon solid solution can be effectively controlled by adjusting the heat treatment temperature. When the iron content is low, the heat treatment temperature can be increased to accelerate the iron-carbon solid solution, increase the etching degree, and increase the pore size. When the iron content is high, the heat treatment temperature can be lowered to avoid excessive etching.

[0026] Furthermore, the hierarchical pores (nano / micro pores) prepared by the present invention. Among them, nanopores can reduce the conductivity of graphene oxide, improve the impedance matching performance, increase the specific surface area of ​​the material, reduce the conductivity of reduced graphene oxide, and improve the impedance matching performance. At the same time, the nanopores can be considered as gas / solid interfaces, and loads are easily accumulated at the interface, thereby leading to interface polarization, which enhances the polarization relaxation ability of the material. In addition, nanopores help to resist the re-deposition of reduced graphene oxide. The micron pore structure can be used as an "effective medium" to improve the impedance matching characteristics of the material, can induce multiple reflections of electromagnetic waves, and extend the propagation path of electromagnetic waves inside the material, thereby enhancing its loss of electromagnetic waves.

[0027] The present invention also discloses a porous reduced graphene oxide aerogel / resin absorbing material, which is a porous reduced graphene oxide aerogel / resin composite material with wide temperature range absorbing performance. When the thickness is 2.75 mm, the effective absorption bandwidth is 4.2 GHz, covering the entire X-band, and the minimum reflection loss value is -41.6 dB. It exhibits excellent X-band absorbing performance at 323-523 k, and can almost always cover the entire X-band. It meets the performance requirements of "thin, wide, light, strong" and low dielectric temperature dependence. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Optical photographs of aerogel materials prepared in Examples 1-3, (a) is the graphene oxide aerogel in Example 1, (b) is the porous reduced graphene oxide aerogel in Example 1, (c) is the porous reduced graphene oxide aerogel in Example 2, and (d) is the porous reduced graphene oxide aerogel in Example 3.

[0029] Figure 2 Scanning electron microscope photos of aerogel materials prepared in Examples 1-3, (a) is the graphene oxide in Example 1, (b) is the porous reduced graphene oxide in Example 1, (c) is the porous reduced graphene oxide in Example 2, and (d) is the porous reduced graphene oxide in Example 3.

[0030] Figure 3 This is a scanning electron microscope photograph of the porous reduced graphene oxide aerogel / phenolic resin composite material prepared in Example 2.

[0031] Figure 4 This is a wide temperature range wave absorption performance diagram of different porous reduced graphene oxide aerogel / phenolic resin composite materials prepared in Example 2;

[0032] Among them, the thickness of Figure (a) is 2.75mm; the thickness of Figure (b) is 3.05mm; the thickness of Figure (c) is 2.95; the thickness of Figure (d) is 2.85mm; and the thickness of Figure (e) is 2.80mm. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0034] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0037] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0038] The present invention discloses a method for preparing a porous reduced graphene oxide aerogel / resin composite material with wide temperature range wave absorbing performance, which specifically comprises the following steps:

[0039] Step 1, graphene oxide solution preparation: weighing graphene oxide slurry, adding it to deionized water, and obtaining a uniformly dispersed graphene oxide aqueous solution by magnetic stirring;

[0040] In this process, graphene oxide slurry is used as a raw material, so that the graphene oxide aqueous solution has good dispersibility.

[0041] Step 2, preparation of graphene oxide aerogel: adding ferric nitrate nonahydrate to the graphene oxide aqueous solution prepared in step 1, stirring the two by magnetic stirring to make them evenly mixed, adding ammonia water to adjust the pH value of the solution, and freeze drying to obtain Fe-loaded aerogel. 3+ Graphene oxide aerogel;

[0042] Step 3, preparation of porous reduced graphene oxide aerogel: placing the graphene oxide aerogel prepared in the step into a tubular furnace, heating and keeping the temperature under argon atmosphere to obtain a loaded Fe 3+ The reduced graphene oxide aerogel was then soaked in hydrochloric acid to remove Fe 3+ , and then dried at 80°C for 2h to obtain porous reduced graphene oxide aerogel;

[0043] Step 4, preparation of resin solution: weigh a certain amount of resin, add it into anhydrous ethanol, and then obtain a uniformly dispersed resin solution by magnetic stirring;

[0044] Step 5, preparation of a porous reduced graphene oxide aerogel / resin composite material with wide temperature range absorbing performance: the porous reduced graphene oxide aerogel prepared in step 3 is placed in the resin solution prepared in step 4 and immersed at normal pressure for 0.5 to 1 hour, then taken out and heated and cured to obtain a porous reduced graphene oxide aerogel / resin composite material with wide temperature range absorbing performance.

[0045] In some embodiments of the present invention, in step 1, the concentration of the graphene oxide solution is 3 to 5 mg / mL.

[0046] In some embodiments of the present invention, in step 1, the magnetic stirring time is 1 hour.

[0047] In some embodiments of the present invention, in step 2, the mass ratio of the ferric nitrate nonahydrate to the graphene oxide in the graphene oxide solution is 0.1 to 0.3. The amount of ferric nitrate nonahydrate should not be too much, as too much will cause the metal salt to agglomerate.

[0048] In some embodiments of the present invention, in step 2, the magnetic stirring time is 1 to 2 hours; the pH value of the solution is 7 to 10; the freezing time is 6 hours, and the drying time is 48 hours.

[0049] In some embodiments of the present invention, the protective atmosphere described in step 3 is argon, the heating rate is 5-10°C / min, the heat treatment temperature is 900-1200°C, the heat treatment time is 1-3h, the hydrochloric acid concentration is 10-30wt.%, the immersion time is 24h, the drying temperature is 80°C, and the drying time is 2h.

[0050] In some embodiments of the present invention, in step 4, the resin is one of phenolic resin, epoxy resin, polyimide resin, bismaleimide resin, silicone resin or cyanate resin.

[0051] It should be noted that during the curing process, different resins use different curing temperatures and curing times.

[0052] As a preferred solution, the resin is phenolic resin, the corresponding curing temperature is 160°C, and the curing time is 1h.

[0053] In some embodiments of the present invention, the resin in step 4 is a phenolic resin, and the concentration of the resin solution is 0.1 to 0.3 g / mL.

[0054] A porous reduced graphene oxide aerogel / resin composite material with wide temperature range wave absorbing performance prepared by the above preparation method, the prepared composite material has a hierarchical pore structure, nano / micron-scale pores are evenly distributed on the reduced graphene oxide sheets, the resin is evenly coated on the graphene surface, the composite material still has a sheet structure, and some graphene will be bonded together.

[0055] The preparation process of the present invention utilizes that graphene oxide is rich in ether bonds, carboxyl groups, hydroxyl groups and carbonyl groups and other oxygen-containing active groups, which are easier to hybridize with other materials. Graphene oxide can provide active sites for metal cations and can serve as a two-dimensional support for anchoring and dispersing metal oxide nanoparticles. Therefore, metal salts can be used as candidate materials for graphene surface pore formers. At present, there are still two main problems in preparing porous reduced graphene oxide absorbing materials by metal salts. One is the uniform dispersion of metal salt / graphene mixed solution. Pure graphene oxide solution is highly negatively charged due to the ionization of carboxyl and phenolic hydroxyl groups, and can form a stable colloid under the action of electrostatic repulsion, thereby avoiding the aggregation of graphene sheets, and the combination of metal cations and graphene is bound to affect the surface charge of graphene, thereby affecting the dispersibility of graphene. Therefore, the present invention solves this problem by regulating the amount of metal salt added and the pH value; second, the strong van der Waals interaction between the reduced graphene oxide sheets will cause the graphene sheets to pile up. Both will make the conductivity of graphene difficult to regulate, which is not conducive to impedance matching and microwave absorption.

[0056] The present invention can adjust the electrical properties of graphene by controlling the graphene preparation process, adjusting the graphene distribution morphology, and compounding with heterogeneous materials, so that it has both strong loss capacity and good impedance matching. The present invention introduces pores into graphene, and the pores are considered to be gas / solid interfaces, which are easy to accumulate charges to generate interface polarization, and the pores on the graphene surface improve the interface polarization. In addition, there is interface relaxation in the heterogeneous system, and compounding graphene with other materials can further increase the heterogeneous interface.

[0057] Regarding the dispersibility of metal salt / graphene mixed solution: The dispersibility of metal salt solution is affected by factors such as ion concentration, temperature and solution pH value. 3+ It is extremely unstable and easily hydrolyzes in aqueous solution to form Fe(OH) 3The precipitation produces agglomeration, and the pH value of its initial precipitation is usually 2.7. By adjusting the concentration of graphene oxide, the acidity of the solution can be enhanced to inhibit Fe 3+ The hydrolysis of Fe 3+ The cations are uniformly adsorbed on the graphene oxide flakes. Experiments have shown that the dispersibility of graphene oxide solution is strongly dependent on pH value, ionic strength, ion type and the number of oxygen-containing functional groups on the surface. The Zeta potential of graphene oxide solution decreases with increasing pH value, which is conducive to the dispersion of graphene; however, high pH will accelerate metal adsorption and reduce the electrostatic repulsion between graphene oxides, resulting in Zeta potential reversal; in addition, when the oxygen content of graphene is low, the adsorption capacity is weak, and the pH value needs to be increased to enhance the adsorption of metal cations. Based on charge screening, deprotonation of oxygen-containing functional groups under different pH conditions, and adsorption between functional groups and metal cations, under the coupling of multiple influencing factors, appropriate ammonia water should be added until the pH value of the solution is stabilized between 7 and 10, so that the graphene oxide is uniformly dispersed. At this time, Fe 3+ In situ generation of cations Fe(OH) 3 Crystals. For the stacking problem of reduced graphene oxide: constructing a three-dimensional porous microstructure is an effective strategy to alleviate the stacking of reduced graphene oxide. The aerogel material prepared by freeze-drying technology has excellent properties such as high porosity, low density, rich pore structure and high specific surface area. This three-dimensional porous structure has unique advantages in optimizing impedance matching, building a conductive network and increasing multiple reflections. Therefore, freeze-drying process can be used to stabilize graphene dispersion. Combined with heat treatment process, the reduction of graphene oxide is completed, and the etching of graphene sheets is completed by iron-carbon solid solution reaction.

[0058] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0059] Example 1

[0060] S1. Preparation of graphene oxide solution: 150 mg of graphene oxide slurry was weighed and added into 30 mL of deionized water, and magnetic stirring was performed for 1 h to obtain a uniformly dispersed graphene oxide solution with a concentration of 5 mg / mL;

[0061] S2. Preparation of graphene oxide aerogel: 15 mg of ferric nitrate nonahydrate was weighed and added to the graphene oxide aqueous solution prepared in S1, and magnetically stirred for 1 hour to obtain a uniformly mixed solution, and then ammonia water was added to adjust the pH value of the solution to 9. After magnetic stirring for 0.5 hour, the mixed solution was introduced into a homemade polytetrafluoroethylene mold, placed in a freeze dryer and frozen for 6 hours, and then low-temperature dried for 48 hours to obtain graphene oxide aerogel;

[0062] S3. Preparation of porous reduced graphene oxide aerogel: The graphene oxide aerogel prepared in S2 was placed in a tubular furnace, and heated to 1100°C at a heating rate of 5°C / min under an argon atmosphere and kept at this temperature for 2 hours. During the heat treatment, graphene oxide came into contact with and reacted with iron oxide nanoparticles, and was catalyzed by iron to form Fe 3 C, and in the formed Fe 3 C, and then the aerogel was soaked in 20 wt % hydrochloric acid for 24 h to remove the iron oxide / iron carbide particles to obtain porous reduced graphene oxide aerogel;

[0063] S4. Preparation of resin solution: Weigh 10 g of phenolic resin, add it to 50 mL of anhydrous ethanol, and stir magnetically for 1 h to obtain a uniformly dispersed phenolic resin solution;

[0064] S5. Preparation of porous reduced graphene oxide aerogel / phenolic resin composite material: The porous reduced graphene oxide aerogel prepared in step S3 is placed in the phenolic resin solution prepared in S4, immersed at normal pressure for 1 hour, and then taken out and cured at 160°C for 1 hour to obtain a porous reduced graphene oxide aerogel / phenolic resin composite material.

[0065] Example 2

[0066] S1 is the same as S1 in Example 1;

[0067] S2. Preparation of graphene oxide aerogel: 30 mg of ferric nitrate nonahydrate was weighed and added to the graphene oxide aqueous solution prepared in S1, and magnetically stirred for 1 h to obtain a uniformly mixed solution, and then ammonia water was added to adjust the pH value of the solution to 8. After magnetic stirring for 0.5 h, the mixed solution was introduced into a homemade polytetrafluoroethylene mold, placed in a freeze dryer and frozen for 6 h, and then low-temperature dried for 48 h to obtain graphene oxide aerogel;

[0068] S3 is the same as S3 in Example 1;

[0069] S4 is the same as S4 in Example 1;

[0070] S5 is the same as S5 in Example 1.

[0071] The wide temperature range wave absorption performance of the porous reduced graphene oxide aerogel / phenolic resin composite material prepared in Example 2 was tested using a vector network analyzer and a high-temperature waveguide cavity. The results showed that the composite material achieved full-frequency effective absorption in the X-band when the thickness was 2.75 mm, and the minimum reflection loss value was -41.6 dB@9.15 GHz when the thickness was 3.00 mm.

[0072] Example 3

[0073] S1 is the same as S1 in Example 1;

[0074] S2. Preparation of graphene oxide aerogel: Weigh 45 mg of ferric nitrate nonahydrate and add it to the graphene oxide aqueous solution prepared in S1, stir it magnetically for 1 hour to obtain a uniformly mixed solution, then add ammonia water to adjust the pH value of the solution to 7, stir it magnetically for 0.5 hour, introduce the mixed solution into a homemade polytetrafluoroethylene mold, put it into a freeze dryer and freeze it for 6 hours, and then low-temperature dry it for 48 hours to obtain graphene oxide aerogel;

[0075] S3. Preparation of porous reduced graphene oxide aerogel: The graphene oxide aerogel prepared in S2 was placed in a tubular furnace, and heated to 1000°C at a heating rate of 5°C / min under an argon atmosphere for 2 hours. During the heat treatment, graphene oxide came into contact with and reacted with iron oxide nanoparticles, and was catalyzed by iron to form Fe 3 C, and in the formed Fe 3 C, and then the aerogel was soaked in 20wt% hydrochloric acid for 24h to remove the iron oxide / iron carbide particles to obtain porous reduced graphene oxide aerogel;

[0076] S4 is the same as S4 in Example 1;

[0077] S5 is the same as S5 in Example 1.

[0078] Figure 1 These are optical photographs of aerogel materials prepared in Examples 1-3, (a) is the graphene oxide aerogel in Example 1, (b) is the porous reduced graphene oxide aerogel in Example 1, (c) is the porous reduced graphene oxide aerogel in Example 2, and (d) is the porous reduced graphene oxide aerogel in Example 3. All four groups of samples are three-dimensional porous aerogel materials.

[0079] Figure 2Scanning electron microscope photos of the surface of graphene aerogel sheets prepared in Examples 1-3, (a) is the graphene oxide in Example 1, (b) is the porous reduced graphene oxide in Example 1, (c) is the porous reduced graphene oxide in Example 2, and (d) is the porous reduced graphene oxide in Example 3. As can be seen from the figure, the surface of the graphene oxide sheet is smooth before the pore-forming agent is added. In Example 1, a small number of holes are evenly distributed on the surface of the porous reduced graphene oxide, with a size range of 25-80nm and an average size of 50nm. In Example 2, a large number of holes are distributed on the surface of the porous reduced graphene oxide, with a pore diameter range of 20-90nm and an average diameter of 60nm. In Example 3, the number of holes on the surface of the porous reduced graphene oxide is greatly reduced, and its size range is 20-100nm, with an average size of 65nm. The amount of pore-forming agent added affects the diameter and number distribution of the holes. As the amount of pore-forming agent added increases, the number of holes on the graphene surface increases first and then decreases, and the diameter range of the holes gradually increases. This is because during the heat treatment process, the metal salt nanoparticles aggregate to form large particles due to Ostwald ripening, and larger holes are formed after the heat treatment. It can be seen that when the mass ratio of the nonahydrate ferric nitrate particles to the graphene oxide in the graphene oxide aqueous solution is 0.2, the number of holes generated is the largest and the pore-forming effect is the best.

[0080] Figure 3 The following is a scanning electron microscope photo of the porous reduced graphene oxide aerogel / phenolic resin composite material prepared in Example 2. Under the action of surface tension, the pore diameter range is expanded to 0.4-7.0 μm, forming a hierarchical pore (nano / micro pore) structure, in which the nanopores help to resist the re-deposition of reduced graphene oxide, reduce the conductivity of reduced graphene oxide, improve impedance matching performance, and easily accumulate loads at the interface, thereby causing interface polarization and improving the polarization relaxation ability of the material. The micropore structure can induce multiple reflections of electromagnetic waves, extend the propagation path of electromagnetic waves inside the material, and thus enhance the material's loss of electromagnetic waves.

[0081] Figure 4This is a wide temperature range absorption performance diagram of the porous reduced graphene oxide aerogel / phenolic resin composite material prepared in Example 2. At 323K, the composite material achieves minimum absorption when the thickness is 3mm, and the minimum reflection loss value is -41.60dB@9.15GHz. When the thickness is 2.75mm, the effective absorption bandwidth is 4.2GHz, which can achieve full-frequency absorption in the X-band; as the test temperature rises to 373K, when the thickness is 3mm, the minimum reflection loss value is -46.61dB@10.45GHz, and when the thickness is 3.05mm, the effective absorption bandwidth is 4.01GHz, covering 8.39-12.4GHz; when the temperature rises to 423K, when the thickness is 2.85mm, the minimum reflection loss value is -41.74dB@10.53GHz, when the thickness is 2.95mm, the effective absorption bandwidth is 4.2GHz, covering the entire X-band; when the temperature rises to 473K, when the thickness is 3.2mm, the minimum reflection loss value is -45.21dB@8.2GHz, when the thickness is 2.85mm, the effective absorption bandwidth is 4.2GHz, covering the entire X-band; when the temperature rises to 523K, when the thickness is 2.95mm, the minimum reflection loss value is -62.78dB@8.77GHz, when the thickness is 2.8mm, the effective absorption bandwidth is 4.2GHz, covering the entire X-band. At 323k~523k, the porous reduced graphene oxide aerogel / phenolic resin composite material shows excellent X-band absorbing performance, and can almost always cover the entire X-band, indicating that the composite material has low dielectric temperature dependence.

[0082] Example 4

[0083] In this embodiment, the heat treatment temperature in S3 is 900° C., the heat treatment time is 3 h, and the rest is the same as in Embodiment 1.

[0084] Example 5

[0085] In this embodiment, the heat treatment temperature in S3 is 1200° C., the heat treatment time is 1 hour, and the rest is the same as in Embodiment 1.

[0086] Example 6

[0087] In this embodiment, in S4, 5 g of epoxy resin was weighed and added to 50 mL of anhydrous ethanol, and the rest was the same as in Example 1.

[0088] Example 7

[0089] In this embodiment, in S4, 15 g of organic silicone resin was weighed and added to 50 mL of anhydrous ethanol, and the rest was the same as in Example 1.

[0090] Example 8

[0091] In this embodiment, in S5, the normal pressure impregnation time is 0.5 h, and the rest is the same as in Example 1.

[0092] Example 9

[0093] In this embodiment, in S1, the amount of graphene oxide slurry added is 0 mg, and the rest is the same as in Example 1.

[0094] Example 10

[0095] In this embodiment, in S1, the amount of graphene oxide slurry added is 120 mg, and the rest is the same as in Example 1.

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a porous reduced graphene oxide aerogel / resin absorbing material, characterized in that: The following steps are involved: Step 1, placing graphene oxide slurry in deionized water, and obtaining a graphene oxide aqueous solution by magnetic stirring; Step 2: Place ferric nitrate nonahydrate in a graphene oxide aqueous solution, mix well, add ammonia water to adjust the pH value of the solution, and freeze-dry to obtain a loaded Fe 3+ Graphene oxide aerogel; Step 3: Load Fe 3+ After heat treatment of the graphene oxide aerogel, a reduced graphene oxide aerogel loaded with Fe3C is obtained, and the reduced graphene oxide aerogel loaded with Fe3C is soaked and dried by hydrochloric acid to obtain a porous reduced graphene oxide aerogel; Step 4, placing the porous reduced graphene oxide aerogel in a resin solution, impregnating it at normal pressure, and then curing it to obtain a porous reduced graphene oxide aerogel / resin absorbing material.

2. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 1, the concentration of the graphene oxide aqueous solution is 3-5 mg / mL.

3. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 2, the mass ratio of the ferric nitrate nonahydrate to the graphene oxide in the graphene oxide aqueous solution is 0.1 to 0.

3.

4. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 2, the pH value of the solution is adjusted to 7-10.

5. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 3, the heat treatment temperature is 900-1200° C., and the heat treatment time is 1-3 hours.

6. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 3, the concentration of hydrochloric acid is 10-30wt.%, the soaking time is 24h, the drying temperature is 80°C, and the drying time is 2h.

7. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 4, the solvent of the resin solution is anhydrous ethanol, and the concentration of the resin solution is 0.1 to 0.3 g / mL.

8. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 4, the normal pressure impregnation time is 0.5 to 1 hour.

9. The method for preparing a porous reduced graphene oxide aerogel / resin absorbing material according to claim 1, characterized in that: In step 4, the curing temperature is 160° C. and the curing time is 1 hour.

10. A porous reduced graphene oxide aerogel / resin absorbing material prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The invention comprises a graphene sheet layer, wherein the graphene sheet layer is coated with resin and has nano-scale pores and micro-scale pores distributed on the graphene sheet layer.

Citation Information

Patent Citations

  • Atmospheric pressure drying preparation method of anisotropic graphene aerogel and heat-conducting composite material of anisotropic graphene aerogel

    CN116553532A

  • Preparation of graphene oxide aerogel beads and applications thereof