Low-carbon-emission environment-friendly light-cured silicon-based release agent and preparation method thereof
By modifying the combination of renewable raw materials such as epoxy castor oil and polydimethylsiloxane and acrylate, solvent-free low-carbon emission photocuring silicon-based release agent is prepared, solving the carbon emission of traditional release agents and The problem of resource consumption achieves rapid curing and efficient release force.
Patent Information
- Application Number
- CN202411113454.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
The raw materials of traditional acrylate release agents mainly rely on fossil resources, resulting in increased carbon emissions and resource consumption. Renewable and environmentally friendly raw materials need to be replaced to reduce carbon emissions.
Using renewable raw materials such as modified epoxy castor oil and polydimethylsiloxane, combined with acrylate and photoinitiators, low-carbon emissions and environmentally friendly photocuring silicon-based release agents are prepared through solvent-free photocuring technology to reduce the Use of fossil raw materials.
It achieves low carbon emissions, rapid curing and high release force, reduces the amount of acrylate, and is suitable for industrial production.
Smart Images

Figure BDA0004992963340000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of release agents, and in particular relates to a low-carbon emission, environment-friendly photocurable silicon-based release agent and a preparation method thereof. Background Art
[0002] UV curing technology is a new environmentally friendly technology based on photochemical theory. The reaction mechanism is that the photoinitiator in the UV resin system absorbs ultraviolet radiation energy and splits into active groups. These active groups can trigger the cross-linking reaction of the resin containing photosensitive functional groups in a very short time to form polymers. Due to the characteristics of UV curing resins such as no solvent, low power consumption, fast curing, low cost, and low process temperature, it has broadened the application range of polymer materials and is widely used in biomedicine, coatings, aerospace, mold design, etc.
[0003] Among many photocurable resins, acrylate is a high molecular polymer with excellent performance. It has the advantages of fast curing, good compatibility with diluents, good resilience, and good wear resistance. Although the release agent prepared by acrylate can adopt green and environmentally friendly photocuring technology, and the photocurable release agent can be used without solvent, which significantly reduces carbon emissions. However, the raw materials of traditional acrylates are basically fossil raw materials. Considering that non-renewable resources such as oil and natural gas are constantly being consumed, the natural supply is limited, and the cost is increasing, it is crucial to use renewable natural materials to replace or partially replace fossil raw materials.
[0004] Therefore, it is urgent to reduce the amount of acrylate used and use renewable and environmentally friendly raw materials to prepare new release agents to further reduce carbon emissions. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a low-carbon emission environmentally friendly photocurable silicone-based release agent and a preparation method thereof. The photocurable silicone-based release agent prepared by the present invention does not use solvents, adopts renewable raw materials and reduces the amount of acrylate, reduces the use of fossil raw materials, and is conducive to reducing carbon emissions.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a low-carbon emission and environmentally friendly photocurable silicone-based release agent, comprising the following raw materials in parts by weight:
[0008] 20-40 parts of modified epoxy castor oil, 20-40 parts of polydimethylsiloxane, 10-20 parts of ethyl acrylate, 1-5 parts of vinyl acetate, 1-5 parts of vinyl acetate, 1-5 parts of acrylic acid, 1-3 parts of photoinitiator, 1-3 parts of flame retardant, and 1-3 parts of leveling agent.
[0009] Preferably, the preparation method of the modified epoxidized castor oil is:
[0010] 1) Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated, and hydrogen peroxide solution is gradually added dropwise to react at a constant temperature to obtain epoxy castor oil;
[0011] 2) Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated, and diisocyanate and dibutyltin dilaurate are added to react at a constant temperature to obtain modified epoxy castor oil.
[0012] Preferably, in step 1), the molar ratio of castor oil, formic acid and hydrogen peroxide is 0.5-1.5:1-3:0.5-1.5; and the amount of concentrated sulfuric acid added is 5-8 wt % of the castor oil.
[0013] Preferably, in step 1), the heating temperature is 40-50° C. and the constant temperature reaction time is 3-5 h.
[0014] Preferably, in step 2), the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate and dibutyltin dilaurate is 1:8-12:5-8:6-10:0.1-0.5.
[0015] Preferably, the heating temperature in step 2) is 60-70° C. and the constant temperature reaction time is 2-3 h.
[0016] Preferably, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenylketone, diaryl iodonium salt or triaryl sulfonium salt.
[0017] Preferably, the flame retardant is tris(2,3-dibromopropyl) phosphate, tris(2,3-dichloropropyl) phosphate, N-hydroxymethyl-3-(dimethylphosphinoyl)propionamide or 1-oxo-4-hydroxymethyl-2,6,7-oxabicyclo[2,2,2]octane.
[0018] Preferably, the leveling agent is a water-based silicone leveling agent.
[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned low-carbon emission and environmentally friendly photocurable silicone-based release agent, characterized in that it comprises the following preparation method:
[0020] 1) Weighing each raw material according to the weight portion;
[0021] 2) uniformly mixing modified epoxy castor oil, polydimethylsiloxane, vinyl acetate and vinyl acetate to obtain component A;
[0022] 2) Ethyl acrylate, acrylic acid, photoinitiator, flame retardant and leveling agent are uniformly mixed to obtain component B;
[0023] 3) Component A and component B are mixed evenly at 30-50° C. to obtain a low-carbon emission, environmentally friendly, light-curable silicone-based release agent.
[0024] Beneficial technical effects:
[0025] 1. The light-curing silicone-based release agent prepared by the present invention does not use solvents, adopts renewable raw materials and reduces the amount of acrylate, reduces the use of fossil raw materials, and is conducive to reducing carbon emissions.
[0026] 2. The release agent prepared by the present invention has good light curing effect and fast speed, and has good release force and residual adhesion rate after film formation.
[0027] 3. The release agent prepared by the present invention has a wide range of raw materials, a simple preparation method, and is suitable for industrial production. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0030] The present invention provides a low-carbon emission and environment-friendly light-curable silicone-based release agent, comprising the following raw materials in parts by weight:
[0031] 20-40 parts of modified epoxy castor oil, 20-40 parts of polydimethylsiloxane, 10-20 parts of ethyl acrylate, 1-5 parts of vinyl acetate, 1-5 parts of vinyl acetate, 1-5 parts of acrylic acid, 1-3 parts of photoinitiator, 1-3 parts of flame retardant, and 1-3 parts of leveling agent.
[0032] Further preferably, the weight parts of the raw materials are: 25-35 parts of modified epoxy castor oil, 25-35 parts of polydimethylsiloxane, 12-15 parts of ethyl acrylate, 2-3 parts of vinyl acetate, 2-3 parts of vinyl acetate, 2-3 parts of acrylic acid, 1-3 parts of photoinitiator, 1-3 parts of flame retardant, and 1-3 parts of leveling agent.
[0033] Preferably, the preparation method of the modified epoxidized castor oil is:
[0034] 1) Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated, and hydrogen peroxide solution is gradually added dropwise to react at a constant temperature to obtain epoxy castor oil;
[0035] 2) Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated, and diisocyanate and dibutyltin dilaurate are added to react at a constant temperature to obtain modified epoxy castor oil.
[0036] Castor oil is a triglyceride of fatty acids, which exists in castor seeds, with a mass fraction of 35% to 57%. Castor is one of the world's top ten oil crops, an important industrial raw material, and is known as renewable "petroleum". Each triglyceride of castor oil contains about 2.7 hydroxyl groups and 3 unsaturated double bonds, and the mass fraction of castor oil hydroxyl is 4.94%. By preparing epoxy castor oil and modifying it with silicone, it is suitable as a component of a photocurable release agent, which can be quickly cured to form a coating under ultraviolet light.
[0037] Preferably, in step 1), the molar ratio of castor oil, formic acid and hydrogen peroxide is 0.5-1.5:1-3:0.5-1.5, and more preferably the molar ratio is 1:2:1; the amount of concentrated sulfuric acid added is 5-8wt% of the castor oil, and more preferably 6wt%.
[0038] Preferably, the heating temperature in step 1) is 40-50°C, more preferably 45°C; the constant temperature reaction time is 3-5h, more preferably 4h.
[0039] Preferably, in step 2), the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate and dibutyltin dilaurate is 1:8-12:5-8:6-10:0.1-0.5, more preferably 1:10:6:8:0.3.
[0040] Preferably, the heating temperature in step 2) is 60-70°C, more preferably 65°C; the constant temperature reaction time is 2-3h, more preferably 2.5h.
[0041] Preferably, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenylketone, diaryl iodonium salt or triaryl sulfonium salt.
[0042] Preferably, the flame retardant is tris(2,3-dibromopropyl) phosphate, tris(2,3-dichloropropyl) phosphate, N-hydroxymethyl-3-(dimethylphosphinoyl)propionamide or 1-oxo-4-hydroxymethyl-2,6,7-oxabicyclo[2,2,2]octane.
[0043] Preferably, the leveling agent is a water-based organosilicon leveling agent, and more preferably a water-based alkyl-modified organosiloxane.
[0044] In a second aspect, the present invention provides a method for preparing the above-mentioned low-carbon emission and environmentally friendly photocurable silicone-based release agent, characterized in that it comprises the following preparation method:
[0045] 1) Weighing each raw material according to the weight portion;
[0046] 2) uniformly mixing modified epoxy castor oil, polydimethylsiloxane, vinyl acetate and vinyl acetate to obtain component A;
[0047] 2) Ethyl acrylate, acrylic acid, photoinitiator, flame retardant and leveling agent are uniformly mixed to obtain component B;
[0048] 3) Component A and component B are mixed evenly at 30-50° C. to obtain a low-carbon emission, environmentally friendly, light-curable silicone-based release agent.
[0049] Example 1
[0050] This embodiment provides a low-carbon emission and environmentally friendly light-curable silicone-based release agent, comprising the following preparation steps:
[0051] 1) Preparation of modified epoxy castor oil:
[0052] Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated to 45° C., and hydrogen peroxide solution is gradually added dropwise for constant temperature reaction for 4 hours to obtain epoxy castor oil, wherein the molar ratio of castor oil, formic acid and hydrogen peroxide is 1:2:1; and the amount of concentrated sulfuric acid added is 6wt%.
[0053] Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated to 65°C, and diisocyanate and dibutyltin dilaurate are added and reacted at a constant temperature for 2.5 hours to obtain modified epoxy castor oil, wherein the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate and dibutyltin dilaurate is 1:10:6:8:0.3.
[0054] 2) 30 parts of modified epoxy castor oil, 30 parts of polydimethylsiloxane, 3 parts of vinyl acetate and 3 parts of vinyl acetate were uniformly mixed to obtain component A;
[0055] 3) 12 parts of ethyl acrylate, 2 parts of acrylic acid, 2 parts of 2-hydroxy-2-methyl-1-phenylacetone, 2 parts of tris(2,3-dibromopropyl) phosphate, and 2 parts of water-based alkyl-modified organosiloxane were mixed uniformly to obtain component B;
[0056] 4) Component A and component B are mixed at 40° C. for 1.5 h to obtain a low-carbon emission, environmentally friendly, photocurable silicone-based release agent.
[0057] Example 2
[0058] This embodiment provides a low-carbon emission and environmentally friendly light-curable silicone-based release agent, comprising the following preparation steps:
[0059] 1) Preparation of modified epoxy castor oil:
[0060] Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated to 40° C., and hydrogen peroxide solution is gradually added dropwise for constant temperature reaction for 3 hours to obtain epoxy castor oil, wherein the molar ratio of castor oil, formic acid and hydrogen peroxide is 0.5:1:0.5; and the amount of concentrated sulfuric acid added is 5wt% of the castor oil.
[0061] Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated to 60°C, and diisocyanate and dibutyltin dilaurate are added and reacted at a constant temperature for 2 hours to obtain modified epoxy castor oil, wherein the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate and dibutyltin dilaurate is 1:8:5:6:0.1.
[0062] 2) 20 parts of modified epoxy castor oil, 20 parts of polydimethylsiloxane, 1 part of vinyl acetate and 1 part of vinyl acetate were uniformly mixed to obtain component A;
[0063] 3) 10 parts of ethyl acrylate, 1 part of acrylic acid, 1 part of 1-hydroxycyclohexyl phenyl ketone, 1 part of N-hydroxymethyl-3-(dimethylphosphinoyl)propionamide, and 1 part of water-based alkyl-modified organosiloxane were mixed uniformly to obtain component B;
[0064] 4) Component A and component B are mixed at 30° C. for 1 hour to obtain a low-carbon emission, environmentally friendly, photocurable silicone-based release agent.
[0065] Example 3
[0066] This embodiment provides a low-carbon emission and environmentally friendly light-curable silicone-based release agent, comprising the following preparation steps:
[0067] 1) Preparation of modified epoxy castor oil:
[0068] Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated to 50° C., and hydrogen peroxide solution is gradually added dropwise for constant temperature reaction for 5 hours to obtain epoxy castor oil, wherein the molar ratio of castor oil, formic acid and hydrogen peroxide is 1.5:3:1.5; and the amount of concentrated sulfuric acid added is 8wt% of the castor oil.
[0069] Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated to 70°C, and diisocyanate and dibutyltin dilaurate are added and reacted at a constant temperature for 3 hours to obtain modified epoxy castor oil, wherein the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate and dibutyltin dilaurate is 1:12:8:10:0.5.
[0070] 2) 40 parts of modified epoxy castor oil, 40 parts of polydimethylsiloxane, 5 parts of vinyl acetate and 5 parts of vinyl acetate were uniformly mixed to obtain component A;
[0071] 3) 20 parts of ethyl acrylate, 5 parts of acrylic acid, 3 parts of diaryliodonium salt, 3 parts of tris(2,3-dibromopropyl) phosphate, and 3 parts of water-based alkyl-modified organosiloxane were mixed uniformly to obtain component B;
[0072] 4) Component A and component B are mixed at 50° C. for 2 hours to obtain a low-carbon emission, environmentally friendly photocurable silicone-based release agent.
[0073] Experimental Example 1
[0074] The photocurable silicone-based release agent prepared in Example 1-3 was coated on a PET film with a thickness of 50 μm, the coating thickness was controlled to be 500 nm, and was cured by irradiation with a UV lamp at 365 nm.
[0075] Refer to GB / T 25256-2010 for room temperature peeling force test: 25mm wide MY2G standard test tape is attached to the test surface of the release material to make a test strip, and a 2kg standard pressure roller is used to reciprocate and roll the test strip for 3 times, and the test strip is left to stand for 20 minutes. The release material is fixed, and the standard test tape is stretched with a tensile machine at a peeling angle of 180° and a peeling speed of 300mm / min to measure the room temperature peeling force, and then the test strip is prepared in the same way and left to stand at 100℃ for 12 hours and then measured in the same way.
[0076] Refer to GB / T 25256-2010 for residual rate test: stick the standard tape peeled off in the peeling force test back on the steel plate, and roll it back and forth 3 times with a 2kg standard roller. Leave it in an environment with room temperature of 23℃ and relative humidity of 50% for 20 minutes, then use a tensile testing machine to peel it 180° at a speed of 300mm / min, and get the test value L1.
[0077] Take a new MY2G standard test tape that has not been in contact with the release material and stick it on the steel plate. Use a 2kg standard roller to reciprocate and roll it three times. Place it in an environment with room temperature of 23°C and relative humidity of 50% for 20 minutes, peel it 180° at 300mm / min, and record the value L0. Residual adhesion rate = L1 / L0×100%.
[0078] The test results are shown in Table 1.
[0079] Table 1 Performance test table
[0080]
[0081] The photocurable silicone-based release agent obtained in Examples 1-3 reduces the amount of acrylate used by adopting renewable modified epoxy castor oil, thereby reducing the use of fossil raw materials and reducing carbon emissions. At the same time, no solvent is required during the preparation process, which reduces pollution. In addition, the photocurable silicone-based release agent obtained has a fast photocuring speed, and the centrifugal force, high temperature resistance, and residual rate are all at a high level.
[0082] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A low-carbon emission and environmentally friendly light-curable silicone-based release agent, characterized in that: The invention comprises the following raw materials in parts by weight: 20-40 parts of modified epoxy castor oil, 20-40 parts of polydimethylsiloxane, 10-20 parts of ethyl acrylate, 1-5 parts of vinyl acetate, 1-5 parts of vinyl acetate, 1-5 parts of acrylic acid, 1-3 parts of photoinitiator, 1-3 parts of flame retardant, and 1-3 parts of leveling agent.
2. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 1, characterized in that: The preparation method of the modified epoxidized castor oil is: 1) Castor oil, formic acid and concentrated sulfuric acid are uniformly mixed and heated, and hydrogen peroxide solution is gradually added dropwise to react at a constant temperature to obtain epoxy castor oil; 2) Epoxy castor oil, hydroxypropyl polysiloxane and isooctyl acrylate are mixed, heated, and diisocyanate and dibutyltin dilaurate are added to react at a constant temperature to obtain modified epoxy castor oil.
3. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 2, characterized in that: In the step 1), the molar ratio of castor oil, formic acid and hydrogen peroxide is 0.5-1.5:1-3:0.5-1.5; and the amount of concentrated sulfuric acid added is 5-8wt% of the castor oil.
4. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 2, characterized in that: In the step 1), the heating temperature is 40-50° C. and the constant temperature reaction time is 3-5 hours.
5. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 2, characterized in that: In the step 2), the mass ratio of epoxy castor oil, hydroxypropyl polysiloxane, isooctyl acrylate, diisocyanate, and dibutyltin dilaurate is 1:8-12:5-8:6-10:0.1-0.
5.
6. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 2, characterized in that: In the step 2), the heating temperature is 60-70° C. and the constant temperature reaction time is 2-3 hours.
7. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 1, characterized in that: The photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenylketone, diaryl iodonium salt or triaryl sulfonium salt.
8. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 1, characterized in that: The flame retardant is tris(2,3-dibromopropyl) phosphate, tris(2,3-dichloropropyl) phosphate, N-hydroxymethyl-3-(dimethylphosphinoyl) propionamide or 1-oxo-4-hydroxymethyl-2,6,7-oxabicyclo[2,2,2]octane.
9. The low-carbon emission and environmentally friendly light-curable silicone-based release agent according to claim 1, characterized in that: The leveling agent is a water-based organic silicon leveling agent.
10. The method for preparing a low-carbon emission and environment-friendly photocurable silicone-based release agent according to any one of claims 1 to 6, characterized in that: The invention comprises the following preparation methods: 1) Weighing each raw material according to the weight portion; 2) uniformly mixing modified epoxy castor oil, polydimethylsiloxane, vinyl acetate and vinyl acetate to obtain component A; 2) Ethyl acrylate, acrylic acid, photoinitiator, flame retardant and leveling agent are uniformly mixed to obtain component B; 3) Component A and component B are mixed evenly at 30-50° C. to obtain a low-carbon emission, environmentally friendly, light-curable silicone-based release agent.