Self-adhesive film, self-adhesive lining bag and preparation method of self-adhesive film and self-adhesive lining bag

By adopting a self-adhesive film design in the lining bag, combining the hierarchical structure of low-density polyethylene, self-adhesive masterbatch, metallocene polyethylene and linear low-density polyethylene, the solution is to solve the problem of the lining bag and the container barrel. The hollowing phenomenon and the difficulty in spraying special packaging materials have achieved high-strength, non-toxic and pollution-free sticky lining bags, ensuring the safety and convenience of the materials.

CN118978872APending Publication Date: 2024-11-19HUNAN YOUPERTH NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185696.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

There is hollowing between the existing lining bag and the container barrel, resulting in material leakage, and the problem cannot be solved by spraying water-based glue for special packaging.

Method used

Using a self-adhesive film, including an adhesive layer, an intermediate layer and an inner layer, a self-adhesive lining bag is formed by the preparation method. The adhesive layer includes low-density polyethylene and self-adhesive masterbatch, and the intermediate layer includes metallocene polyethylene and linear low-density poly Ethylene, the inner layer includes low-density polyethylene, ensuring good fit between the adhesive layer and the inner wall of the container barrel, and is non-toxic and pollution-free.

Benefits of technology

It realizes that the self-adhesive lining bag is not easy to break and leak when filling materials, has moderate viscosity, is easy to spread and use, and is easy to recycle and reuse, solving the problems of hollowing and difficulty in spraying special packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978872A_ABST
    Figure CN118978872A_ABST
Patent Text Reader

Abstract

The invention relates to a self-adhesive film, a self-adhesive lining bag and a preparation method thereof, the self-adhesive film comprises an adhesive layer, a middle layer and an inner layer, the adhesive layer comprises low-density polyethylene and self-adhesive master batch, the middle layer comprises metallocene polyethylene and linear low-density polyethylene, and the inner layer comprises low-density polyethylene. The self-adhesive lining bag has the advantages that the self-adhesive lining bag is high in strength, the tensile strength is larger than 35 MPa, and the self-adhesive lining bag is not prone to breakage and leakage under the condition that materials are filled; the viscosity is moderate, it can be ensured that the viscous layer is well attached to the inner wall of the packaging barrel, unfolding is easy, and operation and use are not affected; and the adhesive layer is not easy to fall off, so that the adhesive layer is convenient to recycle and reuse.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of container barrel liner bags, and in particular to a self-adhesive film, a self-adhesive liner bag and a preparation method thereof. Background Art

[0002] Container barrels are medium-sized bulk containers with the advantages of high strength, light material, corrosion resistance, and easy use. Compared with traditional packaging methods, the use of container barrels can greatly reduce storage and transportation costs. Container barrels are widely used in the chemical, pharmaceutical, coating and other industries, and are one of the main tools for modern storage and transportation of liquid products.

[0003] In order to recycle the container barrel and further reduce the packaging cost, a liner bag is usually placed inside the container barrel, so that the liner bag fits the inner wall of the container barrel, and then the material is filled. After unloading the material, take out the liner bag and put in a new liner bag, and the container barrel can be recycled.

[0004] The existing liner bag is used as follows: roll the liner bag into a strip and load it from the filling port of the container barrel, and inflate the liner bag to expand it; the expanded liner bag fits the inner wall of the container barrel, and then the filling process can be carried out. However, the existing liner bags have some defects. For example, the commonly used liner bags are PE liner bags, which cannot fit tightly against the wall of the container barrel, resulting in a gap between the liner bag and the wall of the container barrel, that is, hollowing. At the hollow position, the liner bag may rupture under the action of the material pressure, so that the material enters between the liner bag and the wall of the container barrel, and the container barrel needs to be cleaned and recycled.

[0005] In order to solve the above problem, some companies will spray water-based glue on the barrel wall of the container barrel to stick to the liner bag to avoid hollowing between the liner bag and the barrel wall. However, this method cannot be used for some special packaging.

[0006] At present, no effective solutions have been proposed for the problems existing in relevant technologies, such as hollowing of liner bags and container barrels, and inability to spray water-based glue on special packaging materials. Summary of the invention

[0007] The purpose of the present application is to provide a self-adhesive film, a self-adhesive liner bag and a preparation method thereof in view of the deficiencies in the prior art, so as to at least solve the problems in the related art of hollowing of liner bags and container barrels and the inability to spray water-based glue on special packaging materials.

[0008] To achieve the above purpose, the technical solution adopted by this application is:

[0009] In a first aspect, the present invention provides a self-adhesive film, comprising:

[0010] A sticky layer, the sticky layer comprising low-density polyethylene and self-adhesive masterbatch;

[0011] An intermediate layer, the intermediate layer is arranged on one side of the adhesive layer, and the intermediate layer comprises metallocene polyethylene and linear low-density polyethylene;

[0012] The inner layer is arranged on one side of the middle layer, and the inner layer comprises low-density polyethylene.

[0013] In some of the embodiments, the thickness of the adhesive layer is 3-6% of the thickness of the self-adhesive film;

[0014] The thickness of the intermediate layer is 85-95% of the thickness of the self-adhesive film;

[0015] The thickness of the inner layer is 10-15% of the thickness of the self-adhesive film.

[0016] In some of the embodiments, the adhesive layer comprises, by weight percentage:

[0017] Low-density polyethylene, 0-60%;

[0018] Self-adhesive masterbatch, 40-100%.

[0019] In some of the embodiments, the intermediate layer comprises, by weight percentage:

[0020] Metallocene polyethylene, 60-80%;

[0021] Linear low-density polyethylene, 20-40%.

[0022] In some of the embodiments, the intermediate layer comprises:

[0023] a first intermediate layer, the first intermediate layer being disposed on one side of the adhesive layer;

[0024] a second intermediate layer, the second intermediate layer being disposed on one side of the first intermediate layer;

[0025] A third intermediate layer is disposed between the second intermediate layer and the inner layer.

[0026] In some of the embodiments, the thickness of the first intermediate layer is 25% to 30% of the thickness of the self-adhesive film;

[0027] The thickness of the second intermediate layer is 30% to 35% of the thickness of the self-adhesive film;

[0028] The thickness of the third intermediate layer is 25% to 30% of the thickness of the self-adhesive film.

[0029] In some embodiments, the thickness of the adhesive layer is 5% of the thickness of the self-adhesive film. In terms of weight percentage, the adhesive layer includes 0% low-density polyethylene and 100% self-adhesive masterbatch, or the adhesive layer includes 20% low-density polyethylene and 80% self-adhesive masterbatch, or the adhesive layer includes 40% low-density polyethylene and 60% self-adhesive masterbatch, or the adhesive layer includes 50% low-density polyethylene and 50% self-adhesive masterbatch, or the adhesive layer includes 60% low-density polyethylene and 40% self-adhesive masterbatch.

[0030] The thickness of the first intermediate layer is 25% of the thickness of the self-adhesive film, and the first intermediate layer comprises 70% of metallocene polyethylene and 30% of linear low-density polyethylene by weight percentage;

[0031] The thickness of the second intermediate layer is 30% of the thickness of the self-adhesive film, and the first intermediate layer comprises 75% of metallocene polyethylene and 25% of linear low-density polyethylene by weight percentage;

[0032] The thickness of the third intermediate layer is 25% of the thickness of the self-adhesive film, and the first intermediate layer comprises 70% of metallocene polyethylene and 30% of linear low-density polyethylene by weight percentage;

[0033] The thickness of the inner layer is 15% of the thickness of the self-adhesive film.

[0034] In a second aspect, the present invention provides a self-adhesive liner bag, comprising:

[0035] The self-adhesive film as described in the first aspect.

[0036] In a third aspect, the present invention provides a method for preparing a self-adhesive film, which is used to prepare the self-adhesive film as described in the first aspect, comprising:

[0037] Preparing a viscous layer, wherein the extrusion temperature for preparing the viscous layer is 150-175° C. and the die temperature is 180-190° C.;

[0038] Prepare an intermediate layer, wherein the extrusion temperature for preparing the intermediate layer is 155-185° C. and the die temperature is 180-190° C.;

[0039] Prepare an inner layer, wherein the extrusion temperature for preparing the inner layer is 150-170° C. and the die head temperature is 180-190° C.;

[0040] The adhesive layer, the middle layer and the inner layer are compounded to form a self-adhesive film.

[0041] In some of the embodiments, including:

[0042] Preparing a viscous layer, wherein the extrusion temperature for preparing the viscous layer is 150-175° C. and the die temperature is 180-190° C.;

[0043] Prepare a first intermediate layer, wherein the extrusion temperature for preparing the first intermediate layer is 155-185° C. and the die temperature is 180-190° C.;

[0044] Preparing a second intermediate layer, wherein the extrusion temperature for preparing the second intermediate layer is 155-185° C. and the die temperature is 180-190° C.;

[0045] Preparing a third intermediate layer, wherein the extrusion temperature for preparing the third intermediate layer is 155-185° C. and the die temperature is 180-190° C.;

[0046] Prepare an inner layer, wherein the extrusion temperature for preparing the inner layer is 150-170° C. and the die head temperature is 180-190° C.;

[0047] The adhesive layer, the first intermediate layer, the second intermediate layer, the third intermediate layer and the inner layer are compounded to form a film.

[0048] In a fourth aspect, the present invention provides a method for preparing a self-adhesive liner bag, which is used to prepare the self-adhesive liner bag as described in the second aspect, comprising:

[0049] The self-adhesive film as described in the first aspect or the self-adhesive film prepared by the preparation method as described in the second aspect is heat-sealed to obtain a self-adhesive liner bag.

[0050] Compared with the related art, the self-adhesive film, the self-adhesive liner bag and the preparation method thereof provided in the embodiment of the present application have the following technical effects:

[0051] 1) High strength, tensile strength> 35MPa, the self-adhesive liner bag is not easy to break and leak when filling materials;

[0052] 2) Moderate viscosity can ensure good adhesion between the adhesive layer and the inner wall of the container, making it easy to unfold without affecting operation;

[0053] 3) Non-toxic and pollution-free, the sticky layer is not easy to fall off, so it is easy to recycle and reuse. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0055] Figure 1 Schematic diagram of a cross section of a self-adhesive film according to an embodiment of the present invention.

[0056] The reference numerals are as follows: 10, adhesive layer; 20, middle layer; 21, first middle layer; 22, second middle layer; 23, third middle layer; 30, inner layer. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0058] Obviously, the drawings described below are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios based on these drawings without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in this field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0059] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those of ordinary skill in the art that the embodiments described in this application may be combined with other embodiments without conflict.

[0060] Unless otherwise defined, the technical terms or scientific terms involved in this application should be understood by people with ordinary skills in the technical field to which this application belongs. The words "one", "a", "a", "the" and the like involved in this application do not indicate a quantitative limitation, and may represent the singular or plural. The terms "include", "comprise", "have" and any of their variations involved in this application are intended to cover non-exclusive inclusions; for example, a process, method, system, product or device that includes a series of steps or modules (units) is not limited to the listed steps or units, but may also include steps or units that are not listed, or may also include other steps or units inherent to these processes, methods, products or devices. The words "connect", "connected", "coupled" and the like involved in this application are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. The "multiple" involved in this application refers to two or more. "And / or" describes the association relationship of associated objects, indicating that there may be three relationships, for example, "A and / or B" can represent: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the objects before and after are in an "or" relationship. The terms "first", "second", "third", etc. involved in this application are only used to distinguish similar objects and do not represent a specific ordering of the objects.

[0061] Example 1

[0062] This embodiment relates to the self-adhesive film, the self-adhesive liner bag and the preparation method thereof of the present invention.

[0063] An exemplary embodiment of the present invention is as follows Figure 1 As shown, a self-adhesive film includes an adhesive layer 10, an intermediate layer 20 and an inner layer 30. The adhesive layer 10 includes low-density polyethylene and self-adhesive masterbatch; the intermediate layer 20 is arranged on one side of the adhesive layer 10, and the intermediate layer 20 includes metallocene polyethylene and linear low-density polyethylene; the inner layer 30 is arranged on one side of the intermediate layer 20, and the inner layer 30 includes low-density polyethylene.

[0064] The thickness of the self-adhesive film is 0.04 mm to 0.075 mm. Preferably, the thickness of the self-adhesive film is 0.05 mm.

[0065] As for the adhesive layer 10, the thickness of the adhesive layer 10 is 3 to 6% of the thickness of the self-adhesive film.

[0066] The adhesive layer 10 comprises, by weight percentage:

[0067] Low-density polyethylene, 0-60%; self-adhesive masterbatch, 40-100%.

[0068] In some embodiments, the low-density polyethylene is 2426H (China National Offshore Oil Corporation Shell Petrochemical Co., Ltd.).

[0069] For the adhesive layer 10, the self-adhesive masterbatch includes a hydrogenated styrene-butadiene block copolymer, a tackifier and an anti-aging agent.

[0070] Preferably, the tackifier is tackifier C5.

[0071] Preferably, the anti-aging agent includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy-4-n-octyloxybenzophenone, and bis-2,2,6,6-tetramethylpiperidinol sebacate.

[0072] Preferably, the mass ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate:2-hydroxy-4-n-octyloxybenzophenone:bis-2,2,6,6-tetramethylpiperidinol sebacate is 2:1:1.

[0073] For the self-adhesive masterbatch, in terms of weight percentage, it includes:

[0074] Hydrogenated styrene-butadiene block copolymer, 50-70%; tackifier, 20-40%; anti-aging agent, 5-10%.

[0075] As for the intermediate layer 20, its thickness is 85 to 95% of the thickness of the self-adhesive film.

[0076] The intermediate layer 20 comprises, by weight percentage:

[0077] Metallocene polyethylene, 60-80%; linear low-density polyethylene, 20-40%.

[0078] In some of the embodiments, the metallocene polyethylene is XP6026ML (ExxonMobil).

[0079] In some of the embodiments, the linear low density polyethylene is 2045G (The Dow Chemical Company).

[0080] Furthermore, the intermediate layer 20 includes a first intermediate layer 21, a second intermediate layer 22 and a third intermediate layer 23. The first intermediate layer 21 is disposed on one side of the adhesive layer 10; the second intermediate layer 22 is disposed on one side of the first intermediate layer 21; and the third intermediate layer 23 is disposed between the second intermediate layer 22 and the inner layer 30.

[0081] As for the first intermediate layer 21, its thickness is 25% to 30% of the thickness of the self-adhesive film.

[0082] As for the second intermediate layer 22, its thickness is 30% to 35% of the thickness of the self-adhesive film.

[0083] As for the third intermediate layer 23, its thickness is 25% to 30% of the thickness of the self-adhesive film.

[0084] For the first intermediate layer 21 , the second intermediate layer 22 , and the third intermediate layer 23 , the weight ratios of the metallocene polyethylene and the linear low-density polyethylene in each of the layers may be the same or different.

[0085] As for the inner layer 30, its thickness is 10 to 15% of the thickness of the self-adhesive film.

[0086] For the self-adhesive film of the present invention, the preparation method thereof comprises:

[0087] Prepare the adhesive layer 10, wherein the extrusion temperature for preparing the adhesive layer 10 is 150-175° C. and the die temperature is 180-190° C.;

[0088] Prepare the middle layer 20, wherein the extrusion temperature for preparing the middle layer 20 is 155-185°C and the die temperature is 180-190°C;

[0089] Prepare the inner layer 30, wherein the extrusion temperature for preparing the inner layer 30 is 150-170°C and the die temperature is 180-190°C;

[0090] The adhesive layer 10, the middle layer 20 and the inner layer 30 are compounded to form a self-adhesive film.

[0091] Furthermore, the preparation method of the self-adhesive film comprises:

[0092] Prepare the adhesive layer 10, wherein the extrusion temperature for preparing the adhesive layer 10 is 150-175° C. and the die temperature is 180-190° C.;

[0093] Prepare the first intermediate layer 21, wherein the extrusion temperature for preparing the first intermediate layer 21 is 155-185°C and the die temperature is 180-190°C;

[0094] Prepare the second intermediate layer 22, wherein the extrusion temperature for preparing the second intermediate layer 22 is 155-185°C and the die temperature is 180-190°C;

[0095] Prepare the third intermediate layer 23, wherein the extrusion temperature for preparing the third intermediate layer 23 is 155-185° C. and the die temperature is 180-190° C.;

[0096] Prepare the inner layer 30, wherein the extrusion temperature for preparing the inner layer 30 is 150-170°C and the die temperature is 180-190°C;

[0097] The adhesive layer 10, the first intermediate layer 21, the second intermediate layer 22, the third intermediate layer 23, and the inner layer 30 are compounded to form a film.

[0098] The self-adhesive film of the present invention can be used to prepare a self-adhesive liner bag. The self-adhesive liner bag is made of the self-adhesive film, the adhesive layer 10 of the self-adhesive film is the outer layer of the self-adhesive liner bag, and the inner layer 30 of the self-adhesive film is the inner layer of the self-adhesive liner bag. The adhesive layer 10 is used to adhere to the inner wall of the container barrel, and the inner layer 30 is used to contact the material.

[0099] For the self-adhesive film of the present invention, its preparation method is as follows:

[0100] The self-adhesive film is heat-sealed to obtain a self-adhesive liner bag.

[0101] The technical effects of the present invention are as follows:

[0102] 1) High strength, tensile strength> 35MPa, the self-adhesive liner bag is not easy to break and leak when filling materials;

[0103] 2) Moderate viscosity can ensure good adhesion between the adhesive layer and the inner wall of the container, making it easy to unfold without affecting operation;

[0104] 3) Non-toxic and pollution-free, the sticky layer is not easy to fall off, so it is easy to recycle and reuse.

[0105] Example 2

[0106] This embodiment relates to a specific implementation of a self-adhesive film and a self-adhesive liner bag.

[0107] In this embodiment, the relevant parameters of the self-adhesive film and the self-adhesive liner bag are as follows:

[0108] The thickness of the self-adhesive liner bag is 0.05mm;

[0109] Adhesive layer 10: thickness 5%, low-density polyethylene 0%, self-adhesive masterbatch 100%;

[0110] First intermediate layer 21: 25% thick, 70% metallocene polyethylene, 30% linear low-density polyethylene;

[0111] The second intermediate layer 22 has a thickness of 30%, 75% of metallocene polyethylene and 25% of linear low-density polyethylene;

[0112] The third intermediate layer 23 has a thickness of 25%, and is composed of 70% metallocene polyethylene and 30% linear low-density polyethylene;

[0113] Inner layer 30: thickness is 15%.

[0114] For the self-adhesive liner bag of this embodiment, the testing parameters are as follows:

[0115]

[0116] Example 3

[0117] This embodiment relates to a specific implementation of a self-adhesive film and a self-adhesive liner bag.

[0118] In this embodiment, the relevant parameters of the self-adhesive film and the self-adhesive liner bag are as follows:

[0119] The thickness of the self-adhesive liner bag is 0.05mm;

[0120] Adhesive layer 10: 5% thickness, 20% low-density polyethylene, 80% self-adhesive masterbatch;

[0121] First intermediate layer 21: 25% thick, 70% metallocene polyethylene, 30% linear low-density polyethylene;

[0122] The second intermediate layer 22 has a thickness of 30%, 75% of metallocene polyethylene and 25% of linear low-density polyethylene;

[0123] The third intermediate layer 23 has a thickness of 25%, including 70% metallocene polyethylene and 30% linear low-density polyethylene; the inner layer 30 has a thickness of 15%.

[0124] For the self-adhesive liner bag of this embodiment, the testing parameters are as follows:

[0125]

[0126] Example 4

[0127] This embodiment relates to a specific implementation of a self-adhesive film and a self-adhesive liner bag.

[0128] In this embodiment, the relevant parameters of the self-adhesive film and the self-adhesive liner bag are as follows:

[0129] The thickness of the self-adhesive liner bag is 0.05mm;

[0130] Adhesive layer 10: thickness 5%, low-density polyethylene 50%, self-adhesive masterbatch 50%;

[0131] The first intermediate layer 21: thickness is 25%, metallocene polyethylene 70%, linear low density polyethylene 30%; the second intermediate layer 22: thickness is 30%, metallocene polyethylene 75%, linear low density polyethylene 25%; the third intermediate layer 23: thickness is 25%, metallocene polyethylene 70%, linear low density polyethylene 30%; the inner layer 30: thickness is 15%.

[0132] For the self-adhesive liner bag of this embodiment, the testing parameters are as follows:

[0133]

[0134] Example 5

[0135] This embodiment relates to a specific implementation of a self-adhesive film and a self-adhesive liner bag.

[0136] In this embodiment, the relevant parameters of the self-adhesive film and the self-adhesive liner bag are as follows:

[0137] The thickness of the self-adhesive liner bag is 0.05mm;

[0138] Adhesive layer 10: thickness 5%, low-density polyethylene 60%, self-adhesive masterbatch 40%;

[0139] The first intermediate layer 21: thickness is 25%, metallocene polyethylene 70%, linear low density polyethylene 30%; the second intermediate layer 22: thickness is 30%, metallocene polyethylene 75%, linear low density polyethylene 25%; the third intermediate layer 23: thickness is 25%, metallocene polyethylene 70%, linear low density polyethylene 30%; the inner layer 30: thickness is 15%.

[0140] For the self-adhesive liner bag of this embodiment, the testing parameters are as follows:

[0141]

[0142] Example 6

[0143] This embodiment relates to a specific implementation of the preparation method.

[0144] In this embodiment, a 5-layer co-extrusion film blowing machine is used to prepare a self-adhesive film, and its preparation parameters are as follows:

[0145] layer Barrel 1 Barrel 2 Barrel 3 Barrel 4 Screen Changer adapter Adhesive layer 10 150 160 170 175 175 175 The first intermediate layer 21 155 165 175 180 185 185 Second intermediate layer 22 155 170 175 185 185 185 The third intermediate layer 23 155 165 175 180 185 185 Inner layer 30 150 165 165 170 170 170 Die head 180 185 190 190

[0146] Example 7

[0147] This embodiment relates to a specific implementation of the preparation method.

[0148] In this embodiment, a 5-layer co-extrusion film blowing machine is used to prepare a self-adhesive film, and its preparation parameters are as follows:

[0149] layer Barrel 1 Barrel 2 Barrel 3 Barrel 4 Screen Changer adapter Adhesive layer 10 150 165 175 175 175 175 The first intermediate layer 21 155 175 180 185 185 185 Second intermediate layer 22 155 175 180 185 185 185 The third intermediate layer 23 155 175 180 185 185 185 Inner layer 30 150 160 170 170 170 170 Die head 180 180 185 190

[0150] Example 8

[0151] This embodiment relates to a specific implementation of the preparation method.

[0152] In this embodiment, a 5-layer co-extrusion film blowing machine is used to prepare a self-adhesive film, and its preparation parameters are as follows:

[0153] layer Barrel 1 Barrel 2 Barrel 3 Barrel 4 Screen Changer adapter Adhesive layer 10 150 165 170 170 175 175 The first intermediate layer 21 155 170 175 185 185 185 Second intermediate layer 22 155 170 175 185 185 185 The third intermediate layer 23 155 170 175 185 185 185 Inner layer 30 150 160 165 170 170 170 Die head 180 185 190 190

[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A self-adhesive film, characterized in that: include: A sticky layer, the sticky layer comprising low-density polyethylene and self-adhesive masterbatch; An intermediate layer, the intermediate layer is arranged on one side of the adhesive layer, and the intermediate layer comprises metallocene polyethylene and linear low-density polyethylene; The inner layer is arranged on one side of the middle layer, and the inner layer comprises low-density polyethylene.

2. The self-adhesive film according to claim 1, characterized in that The thickness of the adhesive layer is 3 to 6% of the thickness of the self-adhesive film; The thickness of the intermediate layer is 85-95% of the thickness of the self-adhesive film; The thickness of the inner layer is 10-15% of the thickness of the self-adhesive film.

3. The self-adhesive film according to claim 1, characterized in that In terms of weight percentage, the adhesive layer comprises: Low-density polyethylene, 0-60%; Self-adhesive masterbatch, 40-100%; and / or In terms of weight percentage, the intermediate layer comprises: Metallocene polyethylene, 60-80%; Linear low-density polyethylene, 20-40%.

4. The self-adhesive film according to any one of claims 1 to 3, characterized in that: The intermediate layer comprises: a first intermediate layer, the first intermediate layer being disposed on one side of the adhesive layer; a second intermediate layer, the second intermediate layer being disposed on one side of the first intermediate layer; A third intermediate layer is disposed between the second intermediate layer and the inner layer.

5. The self-adhesive film according to claim 4, characterized in that The thickness of the first intermediate layer is 25% to 30% of the thickness of the self-adhesive film; The thickness of the second intermediate layer is 30% to 35% of the thickness of the self-adhesive film; The thickness of the third intermediate layer is 25% to 30% of the thickness of the self-adhesive film.

6. The self-adhesive film according to any one of claims 4 to 5, characterized in that: The thickness of the adhesive layer is 5% of the thickness of the self-adhesive film. In terms of weight percentage, the adhesive layer includes 0% low-density polyethylene and 100% self-adhesive masterbatch, or the adhesive layer includes 20% low-density polyethylene and 80% self-adhesive masterbatch, or the adhesive layer includes 40% low-density polyethylene and 60% self-adhesive masterbatch, or the adhesive layer includes 50% low-density polyethylene and 50% self-adhesive masterbatch, or the adhesive layer includes 60% low-density polyethylene and 40% self-adhesive masterbatch; The thickness of the first intermediate layer is 25% of the thickness of the self-adhesive film, and the first intermediate layer comprises 70% of metallocene polyethylene and 30% of linear low-density polyethylene by weight percentage; The thickness of the second intermediate layer is 30% of the thickness of the self-adhesive film, and the first intermediate layer comprises 75% of metallocene polyethylene and 25% of linear low-density polyethylene by weight percentage; The thickness of the third intermediate layer is 25% of the thickness of the self-adhesive film, and the first intermediate layer comprises 70% of metallocene polyethylene and 30% of linear low-density polyethylene by weight percentage; The thickness of the inner layer is 15% of the thickness of the self-adhesive film.

7. A self-adhesive liner bag, characterized in that: include: The self-adhesive film according to any one of claims 1 to 6.

8. A method for preparing a self-adhesive film, for preparing the self-adhesive film as claimed in any one of claims 1 to 6, characterized in that: include: Preparing a viscous layer, wherein the extrusion temperature for preparing the viscous layer is 150-175° C. and the die temperature is 180-190° C.; Prepare an intermediate layer, wherein the extrusion temperature for preparing the intermediate layer is 155-185° C. and the die temperature is 180-190° C.; Prepare an inner layer, wherein the extrusion temperature for preparing the inner layer is 150-170° C. and the die head temperature is 180-190° C.; The adhesive layer, the middle layer and the inner layer are compounded to form a self-adhesive film.

9. The preparation method according to claim 10, characterized in that: include: Preparing a viscous layer, wherein the extrusion temperature for preparing the viscous layer is 150-175° C. and the die temperature is 180-190° C.; Prepare a first intermediate layer, wherein the extrusion temperature for preparing the first intermediate layer is 155-185° C. and the die temperature is 180-190° C.; Preparing a second intermediate layer, wherein the extrusion temperature for preparing the second intermediate layer is 155-185° C. and the die temperature is 180-190° C.; Preparing a third intermediate layer, wherein the extrusion temperature for preparing the third intermediate layer is 155-185° C. and the die temperature is 180-190° C.; Prepare an inner layer, wherein the extrusion temperature for preparing the inner layer is 150-170° C. and the die head temperature is 180-190° C.; The adhesive layer, the first intermediate layer, the second intermediate layer, the third intermediate layer and the inner layer are compounded to form a film.

10. A method for preparing a self-adhesive liner bag, for preparing the self-adhesive liner bag as claimed in claim 7, characterized in that: include: The self-adhesive film according to any one of claims 1 to 6 or the self-adhesive film prepared by the preparation method according to any one of claims 8 to 9 is heat-sealed to obtain a self-adhesive liner bag.