Two-component polyurethane pouring sealant, polyurethane pouring curing adhesive, and preparation method and application of two-component polyurethane pouring sealant and polyurethane pouring curing adhesive
By introducing polyether polyols and aromatic isocyanate oligomers into the polyurethane potting glue, a rigid ring is formed, which solves the problem of insufficient hardness and fold resistance of polyurethane potting glue at high temperature, and achieves high-temperature hardness, fold resistance and resistance of high-temperature hardness, fold resistance and resistance of polyurethane potting glue Taking into account the tear strength to ensure the long-term operation reliability of the air filter cartridge.
Patent Information
- Application Number
- CN202411226100.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
AI Technical Summary
Under high temperature conditions, fine cracks grow into cracks due to vibration, which affects the filtration effect of the air filter cartridge. The prior art is difficult to improve the high-temperature hardness, fold resistance and tear resistance at the same time.
Using two-component polyurethane potting glue, the bifunctional polyether polyol and small molecule diol are introduced into component A, and the aromatic isocyanate oligomer is introduced into component B, forming a rigid ring through curing, which increases the high-temperature hardness and Fold resistance, while meeting viscosity and fluidity requirements.
It achieves the high temperature hardness, fold resistance and tear resistance at high temperature, avoids the growth of fine cracks into cracks, and meets the reliability needs of long-term operation of the air filter cartridge.
Smart Images

Figure BDA0005024600520000131 
Figure BDA0005024600520000141 
Figure BDA0005024600520000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of potting adhesives, in particular to a two-component polyurethane potting adhesive, a polyurethane potting curing adhesive and a preparation method and application thereof. Background Art
[0002] In the process of exhaust gas emission containing smoke or solid particles in many chemical plants, cement plants, thermal power plants, etc., for the protection of the atmospheric environment, the exhaust gas needs to be filtered through an air filter cartridge before it is discharged. The exhaust gas can only be discharged into the atmosphere after it meets the emission standards. In order to meet the exhaust gas emission standards, both ends of the air filter cartridge need to be sealed with glue to prevent the filter cartridge from leaking and affecting the filtering effect.
[0003] Generally speaking, air filter cartridges operate in a relatively high temperature environment, with 60℃~100℃ as one of the main operating environments. Due to the excellent high elasticity and certain temperature resistance of polyurethane, the two-component polyurethane system is widely used in air filter cartridge potting glue at an operating temperature of 60℃~100℃.
[0004] During the operation of the air filter cartridge under working conditions (60℃~100℃), it is impacted by airflow and solid particles in the exhaust gas, causing vibration. This vibration will cause fine cracks in the polyurethane adhesive to grow into cracks due to stress concentration at high temperature, which will lead to the failure of the air filter cartridge to filter. During the long-term use of the polyurethane elastic adhesive, in order to prevent fine cracks from growing into cracks due to stress concentration during vibration, it is necessary to simultaneously improve the high-temperature hardness, high-temperature folding resistance and high-temperature tearing strength of the polyurethane elastic adhesive. However, in the design of the molecular structure, obtaining high-temperature hardness, high-temperature folding resistance and high-temperature tearing strength is to a certain extent a result of mutual confrontation. Specifically, increasing the cross-linking density of the elastic adhesive helps to improve the high-temperature hardness and high-temperature tearing strength of the adhesive after curing; but the increase in cross-linking density will lead to a deterioration in the folding resistance of the adhesive.
[0005] At present, there is an improvement approach: while maintaining the characteristics of the molecular structure with low cross-linking density, the high temperature resistance is improved by introducing a rigid ring structure to avoid the hardness value at high temperature from falling seriously below the target value. The specific scheme of this approach is to use the method of synthesizing prepolymers to add the rigid ring substance to a component of the two-component polyurethane elastic adhesive (component A or component B). And the trifunctional or higher compounds containing rigid rings are introduced into the molecular main chain structure of the polyurethane elastic adhesive through a synthetic reaction, which has a good effect on improving the heat resistance of the adhesive. However, this branched prepolymer containing rigid rings is often unable to be used as a potting adhesive due to its high viscosity and poor fluidity. As a result, it is a major problem in the industry to develop a polyurethane elastomer adhesive for potting adhesives that simultaneously improves high temperature hardness, high temperature folding resistance and tear strength at high temperature. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a two-component polyurethane potting glue, a polyurethane potting curing glue and a preparation method and application thereof. By introducing a difunctional polyether polyol and a small molecule diol into component A, and introducing an aromatic isocyanate-terminated polyurethane oligomer into component B, the two have low viscosity before curing, which can meet the requirements of the potting glue for viscosity and fluidity; and a rigid ring is formed in situ during the curing process, which can simultaneously improve the high-temperature hardness, high-temperature folding resistance and tearing strength of the potting curing glue at high temperature, and can be effectively used in the potting and sealing of air filter cartridges.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a two-component polyurethane potting adhesive, wherein the two-component polyurethane potting adhesive comprises a component A and a component B;
[0009] The component A comprises a polyether polyol, a small molecule diol and a catalyst; the polyether polyol in the component A is a difunctional polyether polyol;
[0010] The B component includes an aromatic isocyanate;
[0011] The molar ratio of the isocyanate groups in component B to the hydroxyl groups in component A in the two-component polyurethane potting adhesive is at least 1.05:1;
[0012] The catalyst includes a trimerization catalyst and a gel catalyst.
[0013] The present invention uses low-viscosity component A and component B to form a rigid ring in situ, thereby taking into account high temperature resistance, high temperature folding resistance, high temperature tearing strength and fluidity during potting. The specific invention mechanism is as follows:
[0014] First of all, the viscosity requirements of the potting compound need to be met. Therefore, component A uses polyether polyol, which has lower viscosity and is more suitable for the processing requirements of the potting compound. Component B uses aromatic isocyanate-terminated polyurethane oligomer, which has moderate viscosity and can meet the viscosity requirements of potting compound.
[0015] Secondly, in order to take into account the high temperature resistance of the potting glue after curing, it is hoped that a rigid ring will be formed in situ during the curing process. Therefore, the polyurethane oligomer in component B contains a difunctional aromatic isocyanate end group. Under the action of a trimerization catalyst, component B self-polymerizes to form an isocyanurate ring. The isocyanurate ring is a rigid ring with high thermal stability, which can significantly improve the high temperature hardness of the potting glue after curing; and the polyurethane oligomer terminated with aromatic isocyanate in component B has good aromatic heat resistance, which is more conducive to improving the heat resistance of the potting glue. The molar number of isocyanate groups in component B needs to be a certain degree of excess compared to the molar number of hydroxyl groups in component A to promote the formation of isocyanurate rings. When NCO / OH (the ratio of the molar number of isocyanate groups in component B to the molar number of hydroxyl groups in component A in a two-component polyurethane potting glue) is less than 1.05, the high temperature hardness value is too low, and the hardness and tear strength of the glue are both low, which cannot meet the expected heat resistance requirements.
[0016] Specifically, the molar ratio of isocyanate groups in component B to hydroxyl groups in component A in the two-component polyurethane potting adhesive can be, for example, 1.05:1, 1.06:1, 1.07:1, 1.08:1, 1.1:1, 1.11:1, 1.12:1, 1.15:1, 1.18:1, 1.2:1, 1.22:1, 1.25:1, 1.28:1 or 1.3:1, etc.
[0017] Under the combined action of the trimerization catalyst and the gelation catalyst, and under the condition of excess isocyanate, the A component and the B component undergo a polyurethane curing reaction, and at the same time, the isocyanate group of the B component generates an isocyanurate ring in situ. The gelation catalyst is a necessary catalyst for the cross-curing of the A and B components. The type and content of the gelation catalyst are conventionally adjusted. The appropriate type and content should be selected so that the cup-free time of the reaction system after the A and B components are mixed is preferably 1 minute to 1 minute and 30 seconds (cup-free time at 25°C and 50% RH). The trimerization catalyst is used to catalyze the self-polymerization of the B component to form an isocyanurate ring structure unique to the scheme of the present invention.
[0018] Preferably, the content of the trimerization catalyst in the A component is 100-300 ppm, for example, it can be 100 ppm, 120 ppm, 145 ppm, 160 ppm, 180 ppm, 210 ppm, 230 ppm, 250 ppm, 270 ppm or 300 ppm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0019] The present invention preferably controls the content of the trimerization catalyst within the above range. When the content of the trimerization catalyst is too low, the degree of rigid ring generated by in-situ polymerization is too low. When the content of the trimerization catalyst is too high, there is a problem of too high degree of rigid ring generated by in-situ polymerization.
[0020] Preferably, the viscosity of component A is 100-2000cps, for example, 100cps, 310cps, 520cps, 730cps, 945cps, 1150cps, 1360cps, 1570cps, 1780cps or 2000cps, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0021] Preferably, the viscosity of component B is 100 to 1000 cps, for example, 100 cps, 200 cps, 300 cps, 400 cps, 500 cps, 600 cps, 700 cps, 800 cps, 900 cps or 1000 cps, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0022] Preferably, the viscosity difference between component A and component B is ≤1000cps, for example, it may be 1000cps, 990cps, 980cps, 950cps, 940cps, 900cps, 890cps, 880cps, 850cps, 840cps or 800cps.
[0023] The present invention needs to control the viscosity of component A and component B within the above range to better meet the needs of potting glue; it is known that if the viscosity difference between the two components is too large, there is a risk of uneven mixing of the two components, which in turn leads to deterioration of various properties of the glue. Furthermore, the present invention preferably has a viscosity difference of ≤1000cps between component A and component B to avoid such risks.
[0024] Preferably, by mass fraction, the A component includes 10 to 25 wt% of a small molecule diol, for example, 10 wt%, 12 wt%, 14 wt%, 15 wt%, 17 wt%, 19 wt%, 20 wt% or 25 wt%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0025] The small molecule diol in the present invention mainly provides hydroxyl groups in the subsequent curing process, reacts with the isocyanate groups in component B to form the hard segment of the polyurethane, thereby improving the high temperature hardness. Reasonable control of the content of the small molecule diol can better balance the performance between high temperature hardness and high temperature folding resistance.
[0026] Preferably, the polyether polyol in the A component includes a high molecular weight polyether polyol having a number average molecular weight of 4000 to 12000, for example, 4000, 4880, 5770, 6660, 7550, 8440, 9330, 10220, 11100 or 12000.
[0027] In order to improve the high-temperature folding resistance, the present invention needs to reduce the crosslinking density. Therefore, a high molecular weight bifunctional polyether polyol is used in component A. The use of this type of polyether polyol can reduce the crosslinking density of the cured glue and greatly improve the high-temperature folding resistance of the cured glue.
[0028] The present invention preferably controls the number average molecular weight of the high molecular weight polyether polyol within the above range, which can reduce the subsequent cross-linking of hydroxyl groups with isocyanate in component B, thereby reducing the cross-linking density and improving the high temperature folding resistance of the cured glue.
[0029] Preferably, the high molecular weight polyether polyol accounts for at least 60wt% of the total mass of component A, for example, it can be 60wt%, 62wt%, 65wt%, 67wt%, 68wt%, 69wt%, 70wt%, 72wt%, 75wt%, 78wt%, 80wt% and the like.
[0030] It is preferred to control the content of high molecular weight polyether polyol within the above range. When the content is too high, the soft segment content is too high and the cross-linking density is too low, resulting in insufficient hardness of the potting compound after final curing. When the content is too low, the hard segment content and the cross-linking density are too high, resulting in high hardness of the potting compound, thereby reducing the high temperature folding resistance of the potting compound.
[0031] Preferably, the polyether polyol in the A component further comprises a low molecular weight polyether polyol.
[0032] Preferably, the number average molecular weight of the low molecular weight polyether polyol is 200-2000, for example, 200, 400, 600, 800, 1000, 1200, 1400, 1600, 1800 or 2000, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0033] The introduction of small molecular weight diols in component A contributes to high temperature hardness and high temperature tear strength, but will lead to a decrease in high temperature folding resistance; the introduction of high molecular weight polyether polyols in component A contributes to high temperature folding resistance, but will lead to a decrease in high temperature hardness and high temperature tear strength; the flexibility of the molecular chains of high molecular weight polyether polyols and small molecular weight diols is quite different. By introducing high molecular weight polyether polyols and small molecular weight diols at the same time in the molecular structure design, it is possible to obtain high temperature folding resistance, high temperature hardness and high temperature tear strength, which has a certain effect. However, when low molecular weight polyether polyols are further introduced into component A, the high temperature hardness, high temperature tear strength and high temperature folding resistance of the material can be further improved simultaneously.
[0034] Preferably, the low molecular weight polyether polyol accounts for 5 to 30 wt% of the total mass of component A, for example, it can be 5 wt%, 8 wt%, 11 wt%, 14 wt%, 17 wt%, 19 wt%, 22 wt%, 25 wt%, 28 wt% or 30 wt%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0035] The present invention preferably introduces 5 to 30% of low molecular weight polyether polyol, which can better balance the high temperature folding resistance, tear strength and high temperature hardness of the glue.
[0036] The B component can directly use aromatic isocyanate. When aromatic isocyanate is used, the prior art generally uses a method of adding a surfactant to improve the compatibility of polyol and isocyanate, but such a method is prone to generate bubbles.
[0037] Preferably, the aromatic isocyanate is an aromatic isocyanate-terminated polyurethane oligomer, and the aromatic isocyanate-terminated polyurethane oligomer comprises a difunctional aromatic isocyanate monomer residue, a difunctional polyether polyol residue and a small molecule diol residue.
[0038] The present invention adopts aromatic isocyanate-terminated polyurethane oligomer as component B. Due to the introduction of polyether polyol residues, the aromatic isocyanate-terminated polyurethane oligomer can solve the dispersion problem of components A and B without adding surfactant.
[0039] Preferably, the difunctional polyether polyol residue in the B component is formed by the reaction of isocyanate and a polyether polyol having a number average molecular weight of 200 to 1000, for example, 200, 280, 370, 460, 550, 640, 730, 820, 910 or 1000, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0040] Preferably, the preparation of the aromatic isocyanate-terminated polyurethane oligomer comprises: mixing a difunctional aromatic diisocyanate, a small molecule diol and a low molecular weight polyether polyol to obtain a mixed system and reacting the system to obtain the aromatic isocyanate-terminated polyurethane oligomer.
[0041] Preferably, the water content in the low molecular weight polyether polyol is less than 200 ppm, for example, it can be 199 ppm, 198 ppm, 197 ppm, 195 ppm, 190 ppm, 180 ppm, 170 ppm, 160 ppm, 150 ppm, 140 ppm, 130 ppm, 120 ppm, 110 ppm, 100 ppm, 90 ppm or 50 ppm, etc.
[0042] Preferably, the mass ratio of the difunctional aromatic diisocyanate to the mixed system is 85-95%, for example, it can be 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%, etc.
[0043] Preferably, the mass proportion of the small molecule diol to the mixed system is 0-1%, for example, it can be 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1% or 1.2%, etc.
[0044] Preferably, the mass proportion of the low molecular weight polyether polyol to the mixed system is 4-13%, for example, it can be 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 8%, 9%, 9.5%, 10%, 11%, 12%, 13% or 13.1%, etc.
[0045] Preferably, the NCO content of the aromatic isocyanate-terminated polyurethane oligomer is 25-28%, for example, it can be 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 27.8%, 28% or 28.2%.
[0046] Preferably, in the two-component polyurethane potting adhesive, the molar ratio of the isocyanate groups in the B component to the hydroxyl groups in the A component is at most 1.3:1.
[0047] The ratio of the molar number of isocyanate groups in component B of the present invention to the molar number of hydroxyl groups in component A is 1.05-1.3:1. Within this range, the glue exhibits excellent comprehensive physical properties after curing. When NCO / OH is too high, the generated rigid six-membered ring is excessive, the hardness is too high, and the elasticity is insufficient, which is manifested in poor folding resistance and reduced use value.
[0048] Preferably, the moisture content of component A and component B is independently 0 to 500 ppm, for example, 0 ppm, 50 ppm, 110 ppm, 160 ppm, 220 ppm, 270 ppm, 330 ppm, 380 ppm, 445 ppm or 500 ppm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0049] As is well known in the art, the water content of components A and B should be controlled. Since isocyanate reacts with water, the storage environment of the two-component polyurethane elastic adhesive system should be controlled so that the two-component polyurethane elastic adhesive system will not have colloid quality problems caused by excessive water content during use.
[0050] Preferably, the polyether polyol comprises any one of polyoxypropylene glycol, polyoxyethylene glycol or polyoxypropylene-oxyethylene glycol or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of polyoxypropylene glycol and polyoxyethylene glycol, a combination of polyoxypropylene-oxyethylene glycol and polyoxyethylene glycol, and a combination of polyoxypropylene glycol and polyoxypropylene-oxyethylene glycol.
[0051] Preferably, the mass percentage of ethylene oxide in the polyoxypropylene-oxyethylene glycol is 1.0% to 50%, for example, it can be 1.0%, 6.5%, 11.9%, 17.4%, 22.8%, 28.3%, 33.7%, 39.2%, 44.6% or 50%, etc., but is not limited to the listed values. Other unlisted values within this range are also applicable, preferably 10% to 30%.
[0052] Preferably, the component A also includes an auxiliary agent.
[0053] Preferably, the auxiliary agent includes any one of a defoamer, a desiccant or an antioxidant, or a combination of at least two of them, wherein a typical but non-limiting combination is a combination of a defoamer and a desiccant, a combination of an antioxidant and a desiccant, a combination of a defoamer and an antioxidant, and preferably a combination of a defoamer, a desiccant and an antioxidant.
[0054] The present invention has no special restrictions on the types and proportions of the defoamer, desiccant or antioxidant in the above-mentioned potting glue. Defoamers, desiccant or antioxidants and proportions well known to those skilled in the art can be used, and can also be selected according to the actual process.
[0055] In a second aspect, the present invention provides a polyurethane potting and curing adhesive, wherein the polyurethane potting and curing adhesive is formed by potting and curing the two-component polyurethane potting adhesive described in the first aspect.
[0056] The polyurethane potting and curing glue provided in the second aspect of the present invention is formed by potting and curing the two-component polyurethane potting glue provided in the first aspect, and can have the three advantages of high temperature hardness, high temperature folding resistance and tear strength at high temperature.
[0057] In a third aspect, the present invention provides a method for preparing a polyurethane potting and curing adhesive, wherein the preparation method uses the two-component polyurethane described in the first aspect for potting and curing; the potting and curing comprises the following steps:
[0058] Step 1) Prepare component A and component B according to the component and moisture requirements;
[0059] Step 2) Mixing and pouring: according to the molar ratio of isocyanate groups in component B to hydroxyl groups in component A in the target two-component polyurethane potting glue, the prepared component A and component B are mixed in a vacuum mixer and poured into a mold;
[0060] Step 3) Curing and molding: After pouring, cure at above 60°C for at least 24 hours.
[0061] The potting and curing method provided in the third aspect of the present invention needs to be cured at least 24 hours at a temperature above 60°C to obtain a polyurethane potting and curing adhesive having high temperature hardness, high temperature folding resistance and high temperature tearing strength. The curing temperature can be, for example, 60°C, 62°C, 65°C, 70°C, 72°C or 75°C, etc.; the curing time can be, for example, 24h, 24.5h, 25h, 25.5h, 26h, 26.5h or 27h, etc.
[0062] The present invention has no special restrictions on the configuration method of the A component and the B component. A configuration method familiar to those skilled in the art can be used, and can also be adjusted according to actual conditions.
[0063] Preferably, the mixing and pouring in step 2) is carried out in a protective atmosphere or in a closed condition, illustratively, the protective atmosphere is nitrogen.
[0064] In a fourth aspect, the present invention provides an application of the two-component polyurethane potting adhesive described in the first aspect in the field of potting, preferably in the potting of air filter cartridges.
[0065] The main operating conditions of general air filter cartridges are 60°C to 100°C. The two-component polyurethane potting adhesive provided by the present invention has excellent high-temperature hardness, high-temperature folding resistance and high-temperature tearing strength at this operating temperature after being cured and formed, and will not cause fine cracks to grow into cracks due to stress concentration.
[0066] Compared with the prior art, the present invention has at least the following beneficial effects:
[0067] (1) The viscosity of component A and component B in the two-component polyurethane potting glue provided by the present invention is moderate, which can meet the viscosity requirements of the potting glue, and component A and component B form a rigid ring in situ during the curing process, and the crosslinking density of the two components during curing is low. The polyurethane potting curing glue formed after curing can simultaneously take into account high-temperature hardness, high-temperature folding resistance and tear strength at high temperature. Specifically, after curing, the two-component polyurethane potting glue has a room temperature hardness of more than 50HD, a high-temperature hardness of more than 30HD, a room temperature tear strength of more than 23N / mm, a high-temperature tear strength of more than 12N / mm, and a high-temperature folding resistance of less than 30mm. It can take into account high-temperature hardness, tear strength and folding resistance, and has excellent comprehensive performance;
[0068] (2) The polyurethane potting curing glue provided by the present invention can be used as an elastic potting glue for air filter cartridges at an operating temperature of 60-100°C. It will not cause fine cracks to grow into cracks due to stress concentration, and can meet the reliability requirements of the air filter cartridges for long-term operation under operating conditions. DETAILED DESCRIPTION
[0069] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0070] Terms and Definitions
[0071] The term "residue" refers to any organic structure introduced into a polymer by a condensation reaction or a free radical reaction involving the corresponding monomer. For example, an ethylene glycol residue refers to the organic structure of ethylene glycol entering the polymer through a condensation reaction -O-CH2-CH2-O-.
[0072] The term "trimerization catalyst" refers to a general term for a class of catalysts that can promote the mutual reaction of isocyanate groups to form a six-membered isocyanurate heterocycle, such as potassium acetate and potassium isooctanoate.
[0073] The term "gel catalyst" refers to a class of catalysts that can promote the reaction between isocyanate and active hydrogen-containing compounds to produce gel, such as dibutyltin di(dodecylsulfide).
[0074] Unless otherwise indicated, the numerical ranges listed herein are intended to include the endpoints of the range, and all values within the range, and the endpoints include all approximate numbers, which are rounded to the nearest integer.
[0075] Test Method
[0076] Moisture test: Test the moisture content of component A. The test standard is GB / T12008.6-1989.
[0077] Isocyanate content test: The isocyanate content test in component B refers to ISO14896-2009, using the di-n-butylamine method, and titrating excess di-n-butylamine with hydrochloric acid to determine the isocyanate content of the system.
[0078] Viscosity test: The viscosity of each component was tested at 25°C and 50% RH using a rotational viscometer in accordance with the national standard GB / T265-1988.
[0079] Material hardness evaluation: According to the test standard GB / T2411-2008, the Shore D hardness of the cured elastic rubber block at room temperature (25°C) and high temperature (100°C) was measured respectively.
[0080] Tear resistance test: After the cured elastic rubber sample is conditioned at 25°C and 50RH% for 24 hours, the tear strength of the elastic rubber sample at room temperature and high temperature is measured. The tear strength test is measured in accordance with the standard GB / T529-2008.
[0081] High temperature folding resistance test: Preparation of samples required for folding resistance test: The target size and shape of the mold used is 150mm×150mm×10mm, and a 150mm×150mm×10mm polyurethane elastic rubber block is obtained. Use a blade or utility knife to cut a 10mm deep incision in the direction perpendicular to the side at the midpoint of one side of the rubber block. Put the rubber block with the incision into a 100℃ oven for 2 hours, and then fold the rubber block 180° along the incision direction at 100℃. Keep the folded rubber block for one minute and observe the length of the sample further cracking along the incision. The crack length is used to measure the folding resistance of the glue. The shorter the crack length, the better the folding resistance.
[0082] As a specific embodiment of the present invention, the small molecule diols involved in the present invention include but are not limited to any one of 1,4-butanediol, methyl 1,3-propanediol, neopentyl glycol, ethylene glycol, 1,3-propanediol, diethylene glycol, 1,2-propanediol, cyclohexanediol, 1,5-pentanediol, dipropylene glycol, trimethylpentanediol or butyl ethyl propanediol, or a combination of at least two of them, wherein a typical but non-limiting combination is a combination of 1,4-butanediol and methyl 1,3-propanediol, a combination of neopentyl glycol and methyl 1,3-propanediol, a combination of ethylene glycol and methyl 1,3-propanediol, a combination of 1,4-butanediol and diethylene glycol, a combination of cyclohexanediol and diethylene glycol, and a combination of 1,4-butanediol and 1,5-pentanediol.
[0083] The catalysts involved in the present invention include but are not limited to any one of tertiary amine catalysts, organotin catalysts or carboxylate catalysts, or a combination of at least two of them. The tertiary amine catalyst may be, for example, triethylenediamine, etc.; the organotin catalyst may be, for example, dibutyltin dilaurate and / or di(dodecylsulfide)dibutyltin, etc.; the carboxylate catalyst may be, for example, potassium isooctanoate and / or potassium acetate, etc. The isocyanate involved in the present invention includes but is not limited to any one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), liquefied diphenylmethane diisocyanate (LMDI) or polymethylene polyphenyl isocyanate (PMDI) or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI), a combination of isophorone diisocyanate (IPDI) and diphenylmethane diisocyanate (MDI), and a combination of toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI).
[0084] The raw materials used in the following examples and comparative examples are shown in Table 1.
[0085] Table 1
[0086]
[0087] Examples 1-9 exemplarily list component A and component B in a two-component polyurethane potting compound.
[0088] The configuration process of component A and component B in the following examples 1-9 is as follows:
[0089] Component A: High molecular weight polyether polyol and low molecular weight polyether polyol are mixed evenly in a 500 mL three-necked glass flask with mechanical stirring at room temperature (generally 25°C), then heated to 110°C under vacuum (-0.1MPa) for dehydration for one hour, sampled and tested for moisture content of the material, if the moisture content is less than 200ppm, add activated molecular sieve powder JLH-03-B (mass is 1.0wt% of the mass of component A) to the material, continue stirring under vacuum at 110°C for 30 minutes, then cool to room temperature, add pre-dried small molecule diol, catalyst and other additives (Irganox1010 and ACP-1500) in a nitrogen atmosphere. Continue mixing under nitrogen protection for 10 minutes, then seal and package for standby use.
[0090] Component B: Add low molecular weight polyether polyol into a 500mL three-necked glass flask with mechanical stirring at room temperature, then heat to 110°C under vacuum (-0.1MPa) and stir to dehydrate for one hour, take samples to detect the moisture content of the material, if the moisture content is less than 200ppm, cool to 70°C, add difunctional aromatic diisocyanate under nitrogen protection, and react in a nitrogen atmosphere at 70°C for 30 minutes; then add pre-dried small molecule diol, continue to react in a nitrogen atmosphere at 70°C for 30 minutes, then take samples to detect the NCO content to the target range, cool to room temperature, unload and package for standby use.
[0091] The component configurations of component A and component B of Examples 1 to 6 and 8 to 9, as well as the component viscosities, moisture contents, and NCO contents are shown in Table 2.
[0092] Table 2
[0093]
[0094]
[0095] Example 7
[0096] The preparation process of component A and component B in Example 7 is basically the same as that in Example 1, except that the low molecular weight polyether polyol Voranol 2000LM in component A is completely replaced by high molecular weight polyether polyol Voranol 8000LM, that is, component A does not contain Voranol 2000LM, and Voranol
[0097] The proportion of 8000LM is 80wt%; component B is the same as that in Example 1.
[0098] Comparative Example 1
[0099] The preparation process of component A in comparative example 1 is basically the same as that in example 1, except that the low molecular weight polyether polyol Voranol 2000LM accounts for 30wt% and the high molecular weight polyether polyol Voranol 8000LM accounts for 50wt% in component A; component B is the same as that in example 1.
[0100] Comparative Example 2
[0101] The configuration process of component A in Comparative Example 2 is basically the same as that in Example 1, except that the high molecular weight polyether polyol Voranol 8000LM in component A is completely replaced by low molecular weight polyether polyol Voranol 2000LM, that is, component A does not contain Voranol 8000LM, and the proportion of Voranol 2000LM is 80wt%; component B is the same as in Example 1.
[0102] Comparative Example 3
[0103] The preparation process of component A in comparative example 3 is basically the same as that in example 1, except that the difunctional high molecular weight polyether polyol Voranol 8000LM in component A is completely replaced by trifunctional high molecular weight polyether polyol Wannal 3135; component B is the same as that in example 1.
[0104] Comparative Example 4
[0105] The preparation process of component A in comparative example 4 is basically the same as that in example 1, except that the amount of trimerization catalyst in component A is 50 ppm; component B is the same as that in example 1.
[0106] Comparative Example 5
[0107] The preparation process of component A in comparative example 5 is basically the same as that in example 1, except that the amount of trimerization catalyst in component A is 500 ppm; component B is the same as that in example 1.
[0108] Examples 10-18 respectively use the two-component polyurethane potting glue (component A and component B) of Examples 1-9 for potting and curing to obtain polyurethane potting and curing glue samples; Comparative Examples 6-10 respectively use the two-component polyurethane potting glue (component A and component B) of Comparative Examples 1-5 for potting and curing to obtain polyurethane potting and curing glue comparison samples; Comparative Examples 11-12 both use the two-component polyurethane potting glue (component A and component B) of Example 1 for potting and curing to obtain polyurethane potting and curing glue comparison samples;
[0109] The potting is carried out according to the following process:
[0110] Step 1) preparing component A and component B according to the component and moisture requirements disclosed in Table 3;
[0111] Step 2) Mixing and pouring: The molar ratio of the isocyanate group in component B to the hydroxyl group in component A in the two-component polyurethane potting adhesive is shown in Table 3. The prepared components A and B are mixed in a vacuum mixer and poured into a mold;
[0112] Step 3) Curing and molding: After pouring, cure at 60°C for 24 hours.
[0113] Table 3
[0114]
[0115]
[0116] The potting properties of the two-component polyurethane potting adhesives used in Examples 10-18 and Comparative Examples 6-12 were evaluated, and the room temperature hardness (Shore D), high temperature hardness (Shore D), room temperature tear strength, high temperature tear strength, and high temperature folding resistance of the polyurethane potting curing adhesive samples finally obtained were evaluated. The test results are shown in Table 4:
[0117] Table 4
[0118]
[0119] From Tables 2 to 4, we can see the following points:
[0120] (1) It can be seen from Examples 10 to 18 that the two-component polyurethane potting adhesive provided by the present invention has high potting properties, and the polyurethane potting cured adhesive formed after potting and curing has a room temperature hardness of more than 50HD, a high temperature hardness of more than 30HD, a room temperature tear strength of more than 23N / mm, a high temperature tear strength of more than 12N / mm, and a high temperature folding resistance of less than 30mm. It can take into account high temperature hardness, tear strength and folding resistance, and has excellent comprehensive performance.
[0121] The room temperature hardness requirement for the polyurethane elastic potting glue for industrial air filters is between 50HD and 60HD on the Shore A scale. If the hardness is too low, the tear strength is insufficient, and if the hardness is too high, the glue is too brittle and the folding resistance is insufficient. Within the required hardness range, the higher the tear strength, the better the tear resistance of the glue sample; the folding resistance is manifested in that when the sample is folded in half along the incision at 180°, the shorter the extension length of the incision, the better the folding resistance. Examples 10 to 18 show the performance (including hardness, tear strength and folding resistance) of the rigid structure of the isocyanurate six-membered ring generated in the presence of a trimerization catalyst using a two-component polyurethane potting glue and a two-functional polyether polyol composition when isocyanate (NCO) is excessive. The six-membered rigid ring of isocyanurate improves the hardness retention rate of the glue at high temperatures on the one hand, and forms a locally cross-linked micro-region at the same time, making the polyurethane microphase separation more thorough, thereby greatly improving the comprehensive physical properties of the glue. Elastomers based on these formulations exhibit reasonable high temperature hardness, good tear strength and excellent folding resistance.
[0122] (2) Crosslink density
[0123] A. Effect of adding low molecular weight polyether polyol
[0124] From the comparison between Example 10 and Example 16, it can be seen that the low molecular weight polyether polyol is added in Example 10, and compared with Example 16 without adding the low molecular weight polyether polyol, the finally formed polyurethane potting curing glue has a room temperature hardness of 54HD, a high temperature hardness of 33HD, a room temperature tear strength of 29N / mm, and a high temperature tear strength of 17N / mm, while the room temperature hardness of the polyurethane potting curing glue in Example 16 is 51HD, the high temperature hardness is 30HD, the room temperature tear strength is 23N / mm, and the high temperature tear strength is 12N / mm, which are slightly lower than those in Example 10. This shows that the present invention can further improve the comprehensive performance of the two-component polyurethane potting glue after curing by adding the low molecular weight polyether polyol;
[0125] B. Influence of the proportion of high molecular weight polyether polyols
[0126] By comparing Example 10 with Comparative Examples 6-7, it can be seen that the proportion of high molecular weight polyether polyols in Comparative Examples 6-7 is 50% and 0%, respectively. The proportion of high molecular weight polyether polyols in Comparative Examples 6 and 7 is too low, which ultimately leads to the relative hard segment content and cross-linking density of Comparative Examples 6 and 7 being too high, resulting in the potting compound having a high hardness, thereby reducing the high temperature folding resistance of the potting compound. The final high temperature folding resistance of Comparative Example 6 is as high as 80mm; while in Comparative Example 7, since all low molecular weight polyether polyols are used, the cross-linking density is higher, and the folding resistance of the potting compound after curing is further reduced compared to Comparative Example 6. This shows that the present invention can effectively control the cross-linking density by selecting high molecular weight polyether polyols for cross-linking, thereby taking into account the high temperature folding resistance, high temperature hardness and high temperature tear strength of the potting compound after curing;
[0127] C. Influence of functionality of high molecular weight polyether polyols
[0128] By comparing Example 10 and Comparative Example 8, it can be seen that in Example 10, Voranol 8000LM with two functionalities is used as the high molecular weight polyether polyol. Compared with the trifunctional Wannal 3135 used as the high molecular weight polyether polyol in Comparative Example 8, the crosslinking density in Comparative Example 8 is significantly too high due to the trifunctional active groups, and the hardness of the generated potting glue is high, but the high temperature folding resistance is significantly lower than that of Example 10 (up to 140 mm in Comparative Example 8). This shows that the present invention can improve the comprehensive performance of the potting glue by controlling the number of functionalities of the high molecular weight polyether polyol to 2;
[0129] (3) Generation of rigid loops
[0130] A. Effect of trimerization catalyst dosage
[0131] By comparing Example 10 with Comparative Examples 9 to 10, it can be seen that the dosage of the trimerization catalyst in Comparative Examples 9 to 10 is 50 ppm and 500 ppm, respectively. In the end, too few rigid rings are formed in Comparative Example 9, and the high-temperature hardness and tear strength are both low; the rigid six-membered rings generated in Comparative Example 10 are excessive, the hardness is too high, and the elasticity is insufficient, which is manifested in poor folding resistance (high-temperature folding resistance is 40 mm). This shows that the present invention can effectively control the amount of rigid rings generated by controlling the dosage of the trimerization catalyst within a specific range, thereby taking into account the high-temperature folding resistance, high-temperature hardness and high-temperature tear strength of the potting glue after curing;
[0132] B. Influence of NCO / OH ratio
[0133] By comparing Example 10 with Comparative Examples 11 to 12, it can be seen that in Comparative Example 11, the NCO / OH ratio is 1:1, the -NCO group is basically used for cross-linking reaction, and it is difficult for the remaining -NCO to self-polymerize to form a rigid ring. Therefore, too few rigid rings are formed, and the high-temperature hardness and tear strength are both low; in Comparative Example 12, the NCO / OH ratio is 1.4:1, the remaining -NCO self-polymerizes to form too many rigid rings, the hardness is too high, and the elasticity is insufficient, which is manifested in poor folding resistance (high-temperature folding resistance is as high as 60mm).
[0134] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A two-component polyurethane potting adhesive, characterized in that: The two-component polyurethane potting adhesive comprises component A and component B; The component A comprises a polyether polyol, a small molecule diol and a catalyst; the polyether polyol in the component A is a difunctional polyether polyol; The B component includes an aromatic isocyanate; The molar ratio of the isocyanate groups in component B to the hydroxyl groups in component A in the two-component polyurethane potting adhesive is at least 1.05:1; The catalyst includes a trimerization catalyst and a gel catalyst.
2. The two-component polyurethane potting adhesive according to claim 1, characterized in that: The content of trimerization catalyst in the A component is 100-300 ppm.
3. The two-component polyurethane potting adhesive according to claim 1, characterized in that: The viscosity of the component A is 100 to 2000 cps; Preferably, the viscosity of the B component is 100 to 1000 cps; Preferably, the viscosity difference between the component A and the component B is ≤1000 cps.
4. The two-component polyurethane potting adhesive according to claim 1, characterized in that: Calculated by mass fraction, the component A includes 10 to 25 wt % of small molecule diol.
5. The two-component polyurethane potting adhesive according to claim 1 or 2, characterized in that: The polyether polyol in the A component includes a high molecular weight polyether polyol, and the number average molecular weight of the high molecular weight polyether polyol is 4000 to 12000; Preferably, the high molecular weight polyether polyol accounts for at least 60 wt% of the total mass of component A; Preferably, the polyether polyol in component A further comprises a low molecular weight polyether polyol; Preferably, the number average molecular weight of the low molecular weight polyether polyol is 200 to 2000; Preferably, the low molecular weight polyether polyol accounts for 5 to 30 wt % of the total mass of component A.
6. The two-component polyurethane potting adhesive according to any one of claims 1 to 5, characterized in that: The aromatic isocyanate is an aromatic isocyanate-terminated polyurethane oligomer, and the aromatic isocyanate-terminated polyurethane oligomer contains a difunctional aromatic isocyanate monomer residue, a difunctional polyether polyol residue and a small molecule diol residue; Preferably, the difunctional polyether polyol residue in the B component is formed by the reaction of isocyanate and a polyether polyol having a number average molecular weight of 200 to 1000; Preferably, the preparation of the aromatic isocyanate-terminated polyurethane oligomer comprises: mixing a difunctional aromatic diisocyanate, a small molecule diol and a low molecular weight polyether polyol, and reacting them to obtain the aromatic isocyanate-terminated polyurethane oligomer; Preferably, the water content in the low molecular weight polyether polyol is less than 200 ppm; Preferably, the mass proportion of the difunctional aromatic diisocyanate to the mixed system is 85-95%; Preferably, the mass proportion of the small molecule diol to the mixed system is 0-1%; Preferably, the mass proportion of the low molecular weight polyether polyol to the mixed system is 4 to 13%; Preferably, the NCO content of the aromatic isocyanate-terminated polyurethane oligomer is 25-28%.
7. The two-component polyurethane potting adhesive according to claim 1, characterized in that: The molar ratio of the isocyanate groups in component B to the hydroxyl groups in component A in the two-component polyurethane potting adhesive is at most 1.3:1; Preferably, the moisture content of the component A and the component B is independently 0 to 500 ppm.
8. A polyurethane potting and curing adhesive, characterized in that: The polyurethane potting and curing adhesive is formed by potting and curing the two-component polyurethane potting adhesive according to any one of claims 1 to 7.
9. A method for preparing a polyurethane potting and curing adhesive, characterized in that: Using the two-component polyurethane potting adhesive according to any one of claims 1 to 7 for potting and curing; The potting and curing comprises the following steps: Step 1) Prepare component A and component B according to the component and moisture requirements; Step 2) Mixing and pouring: according to the molar ratio of isocyanate groups in component B to hydroxyl groups in component A in the target two-component polyurethane potting glue, the prepared component A and component B are mixed in a vacuum mixer and poured into a mold; Step 3) Curing and molding: After pouring, cure at above 60°C for at least 24 hours.
10. Use of the two-component polyurethane potting adhesive according to any one of claims 1 to 7 in the field of potting, preferably in the potting of air filter cartridges.