Light-load engine oil complexing agent for improving old oil MRV and preparation method and application of light-load engine oil complexing agent

By adding a light-load engine oil composite agent with a specific ratio to the old oil, the problem of insufficient low-temperature pumping performance of old oil is solved, better low-temperature flow and oxidation resistance are achieved, the engine life is extended, and the engine life is reduced. Production cost.

CN118978947APending Publication Date: 2024-11-19XINXIANG RICHFUL LUBE ADDITIVE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411035504.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing technology cannot effectively improve the low-temperature pumping performance of old oil, resulting in flow restrictions and air entrainment of the engine under low temperature conditions, causing wear, and the aging method is not harsh enough, the catalyst does not have enough aging strength for aging oil, high raw material costs, and economical Poor sex.

Method used

Using a light load engine oil composite agent, including dispersants, detergents, antioxidants, friction modifiers, coagulation reducing agents and neutral base oils, the low-temperature flowability of old oil is improved through specific ratios and processes. and antioxidant properties to reduce costs.

Benefits of technology

Significantly improve the low-temperature pumping performance of old oil, extend the engine service life, reduce production costs, provide better cleanliness and oxidation resistance, reduce component wear, and improve power efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970961870000131
    Figure BDA0004970961870000131
  • Figure BDA0004970961870000132
    Figure BDA0004970961870000132
  • Figure BDA0004970961870000141
    Figure BDA0004970961870000141
Patent Text Reader

Abstract

The invention relates to the technical field of engine oil complexing agents, in particular to a light-load engine oil complexing agent for improving old oil MRV and a preparation method and application of the light-load engine oil complexing agent. The light-load engine oil complexing agent comprises the following components in parts by weight: 35-65 parts of a dispersing agent, 1-20 parts of a clearing agent, 8-15 parts of zinc dialkyl dithiophosphate, 13-28 parts of an antioxidant, 1-5 parts of a friction modifier, 1-4 parts of a pour point depressant and 0.5-5 parts of neutral base oil. The light-load engine oil complexing agent can provide better low-temperature performance protection for a gasoline engine and a small diesel engine, and it is guaranteed that an oil product still has excellent low-temperature fluidity after being used for a period of time; meanwhile, good detergency and oxidation resistance can be provided for a gasoline engine and a small diesel engine, engine oil deterioration is inhibited, and the oil change period is prolonged; and excellent wear resistance can be provided for gasoline engines and small diesel engines, part wear is reduced, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engine oil compounding agents, and in particular to a light-load engine oil compounding agent for improving the MRV of used oil, and a preparation method and application thereof. Background Art

[0002] Engine oil can lubricate and reduce friction, assist in cooling, seal and prevent leakage, prevent rust and corrosion, and reduce shock and buffer. It is known as the "blood" of the car. In terms of oil performance, the SAE J300 automotive engine oil standard has clear requirements for low-temperature cold starting viscosity and low-temperature pumping viscosity. Testing low-temperature cold starting viscosity and low-temperature pumping viscosity is very important, but these performance indicators are all requirements for the low-temperature performance of new oil. After a period of use, the oil will fail to pump at low temperatures. Therefore, for engine oil, it is necessary to examine the low-temperature pumping viscosity of the old oil, that is, the old oil MRV.

[0003] Low-temperature pumping performance reflects the rheological behavior of the engine oil in the oil pump area. The pumping capacity of the engine oil depends on the apparent viscosity under pumping conditions. The reasons for the pumping failure phenomenon are "flow restriction" and "air entrainment". Among them, "flow restriction" is due to the poor fluidity of the oil. When the pump sucks oil, the surrounding oil cannot be replenished in time, resulting in the oil pump inlet being evacuated and forming cavities; "air entrainment" is due to the partial formation of gel by the engine oil under low temperature conditions. When the oil pump pumps the gel, air is easier to enter the oil pump inlet than the gel, causing air entrainment. The air gap will cause the engine's moving friction pair surface to wear and damage in a short period of time, thereby causing certain damage to the engine.

[0004] Therefore, it is crucial to improve the MRV of old engine oil, which will effectively protect the engine and extend its service life.

[0005] The Chinese patent application number CN201610958550.3 discloses a lubricating oil composition and a method for improving the low temperature performance of a lubricating oil. The application examines the effects of the lubricating oil composition on the low temperature performance of new oil and aged oil, respectively, but the aging method is not harsh enough. The aging method involved in the application has the problems of short aging time and low aging temperature. The aging time is 40 hours and the aging temperature is 170°C. At the same time, the MRV temperature of the aged oil test (the MRV temperature of the aged oil test in Table 4 of the application specification is -30°C) is higher than the MRV temperature of the new oil test (the MRV temperature of the new oil test in Table 4 of the application specification is -35°C). The above two points cannot fully guarantee the precision and accuracy of the low temperature pumping performance test of the aged oil. In addition, the lubricating oil composition contains an oil-soluble organic molybdenum friction modifier, which has the problems of high raw material cost and poor economy. Moreover, the catalyst used in the application has low aging strength to the aged oil.

[0006] The Chinese patent application number CN202010905981.X discloses a lubricating oil pour point depressant and a preparation method thereof. The application provides a pour point depressant that can effectively improve the low-temperature pumping viscosity of engine oil, but the pour point depressant is only mixed with the base oil, and the compatibility of the pour point depressant with other components in the composite agent is not investigated. At the same time, its aging method still has the problem of not being harsh enough, that is, the aging method involved in the application is the same as the aging method in the aforementioned application number CN201610958550.3.

[0007] To this end, the present invention provides a light-load engine oil compound for improving the MRV of used oil, and a preparation method and application thereof. Summary of the invention

[0008] Based on this, it is necessary to provide a light-load engine oil compound for improving the MRV of used oil, a preparation method and application thereof in response to the above-mentioned technical problems.

[0009] In order to achieve the above object, the technical solution of the present invention is as follows.

[0010] According to a first aspect of the present invention, a light-load engine oil compound for improving the MRV of used oil is provided, comprising: 35-65 parts by weight of a dispersant, 1-20 parts by weight of a detergent, 8-15 parts by weight of dialkyl dithiophosphate zinc, 13-28 parts by weight of an antioxidant, 1-5 parts by weight of a friction modifier, 1-4 parts by weight of a pour point depressant, and 0.5-5 parts by weight of a neutral base oil, wherein the dispersant is 7-10 parts by weight of boronated polyisobutylene succinimide, 20-45 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, and 7-10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine.

[0011] Furthermore, the boron content of the boronated polyisobutylene succinimide is ≤0.35%, and the nitrogen content of the boronated polyisobutylene succinimide is 1.1-1.4%.

[0012] Furthermore, the dispersant involved in the present invention is composed of a reaction product A of boronated polyisobutylene succinimide, polyisobutylene succinic anhydride and polyene polyamine, and a reaction product B of polyisobutylene succinic anhydride and polyene polyamine. The three materials are maleic anhydride connected to polyisobutylene (i.e., PIB), have good low-temperature dispersibility and high-temperature stability, and mainly function to disperse and solubilize, inhibit the formation of carbon deposits and paint films on engine pistons, and effectively control the increase in gasoline engine oil viscosity.

[0013] Furthermore, the detergent is 6-8 parts by weight of magnesium alkyl salicylate and 4-12 parts by weight of calcium sulfide alkyl phenate.

[0014] Furthermore, the detergent of the present invention is composed of magnesium alkyl salicylate and calcium alkyl phenol sulfide, and its main function is to neutralize the acidic oxidation products and acid value colloids produced by oxidation and incomplete combustion in the oil. At the same time, it has excellent high-temperature cleanliness and thermal stability, and can clean the paint film and sediment on the piston surface in time. The cleaning effect is better after the two are compounded. In addition, magnesium alkyl salicylate can produce less sulfate ash while providing the same base value as calcium alkyl sulfonate, so it can provide better anti-low-speed pre-ignition protection for the engine.

[0015] Furthermore, the zinc dialkyl dithiophosphate is 3-7 parts by weight of bis-octyl alkyl zinc thionate and 4-8 parts by weight of di-secondary alkyl zinc thionate, the zinc content of the bis-octyl alkyl zinc thionate is 8.5-10.5%, and the zinc content of the di-secondary alkyl zinc thionate is 7.3-8.7%.

[0016] Furthermore, the dialkyl zinc dithiophosphate involved in the present invention is composed of dioctyl primary alkyl zinc thiophosphate and di-secondary alkyl zinc thiophosphate, which mainly provides anti-wear performance for oil products. At the same time, it has antioxidant and anti-corrosion properties, prevents wear of cylinders, ring grooves, cams and tappets, and can also prevent bearing corrosion.

[0017] Furthermore, the antioxidant is 5-14 parts by weight of nonyldiphenylamine and 6-14 parts by weight of a phenolic ester antioxidant, and the nitrogen content of the nonyldiphenylamine is 3.2-3.8%.

[0018] Furthermore, the antioxidant involved in the present invention is composed of nonyldiphenylamine and phenolic ester antioxidant, has excellent high-temperature antioxidant property and high-temperature thermal stability, has a significant effect on inhibiting the late oxidation of oil products, and can extend the service life of gasoline engine oil. The antioxidant effect is better after the two are compounded.

[0019] Furthermore, the friction modifier is a polymer of oleylamine and ethylene oxide, and the nitrogen content of the polymer of oleylamine and ethylene oxide is 3.5-4.5%.

[0020] Furthermore, the friction modifier of the present invention is oleylamine and ethylene oxide polymer, which mainly functions to reduce friction between parts and reduce resistance. The mechanism of action is that the mixture contains polar groups, which have strong affinity for metal surfaces and can be strongly adsorbed on the metal surface to form a protective film similar to a cushion, which serves the purpose of separating metals and preventing direct contact between metals, thereby reducing friction and wear, thereby achieving energy-saving effects. In addition, it can effectively prevent the occurrence of excessive oil temperature due to excessive friction, and even oxidation and deterioration of oil products, and the friction modifier has a low cost, which greatly reduces the production cost.

[0021] Furthermore, the pour point depressant is a methacrylate higher alcohol ester copolymer.

[0022] Further, the pour point depressant of the present invention is a methacrylate high-carbon alcohol ester copolymer. It is generally believed that the alkyl side chain of the methacrylate high-carbon alcohol ester copolymer has a similar structure to paraffin hydrocarbons in oil products. The same part is a hydrocarbon chain (non-polar group), which can form a eutectic with paraffin, and the different part (polar group) hinders the further growth of wax crystals. In addition, the active ingredients in the pour point depressant can be adsorbed on the surface of wax crystals, inhibit the growth of wax crystals, change the structure and morphology of wax crystals, and make the wax crystals small and uniform. The pour point depressant can also improve the anti-adhesion between wax crystals and prevent wax crystals from agglomerating to form large wax clusters, thereby achieving the purpose of improving the low-temperature performance of finished oil.

[0023] According to a second aspect of the present invention, there is provided a method for preparing a light-load engine oil compound for improving the MRV of used oil, comprising the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, subsequently cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, subsequently adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining the temperature at 55-60°C, stirring for 2-3 hours, and filtering to obtain the light-load engine oil compound.

[0024] According to a third aspect of the present invention, there is provided a use of a light-duty engine oil compound for improving the MRV of used oil in the lubrication of gasoline engines and small diesel engines.

[0025] The advantages and beneficial effects of the present invention are:

[0026] 1. The light-load engine oil compound of the present invention can provide better low-temperature performance protection for gasoline engines and small diesel engines, ensuring that the oil still has excellent low-temperature fluidity after being used for a period of time.

[0027] 2. The light-load engine oil compound of the present invention can provide good detergency and oxidation resistance for gasoline engines and small diesel engines, inhibit engine oil deterioration, and extend the oil change cycle.

[0028] 3. The light-load engine oil compound of the present invention can provide excellent anti-wear performance for gasoline engines and small diesel engines, reduce component wear and extend service life.

[0029] 4. The light-load engine oil compound of the present invention can provide better friction reduction performance for gasoline engines and small diesel engines, can reduce resistance to a certain extent, improve power, and achieve energy-saving effects.

[0030] 5. The light-load engine oil compound of the present invention adopts relatively low-cost raw materials, and each single agent has good compatibility. While achieving excellent comprehensive performance, it can also greatly reduce the oil blending cost, and has significant economic benefits. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below through specific implementation methods. It should be understood that the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0032] Example 1

[0033] In this embodiment, a light-load engine oil compound for improving the MRV of used oil includes: 35 parts by weight of a dispersant, 28 parts by weight of an antioxidant, 20 parts by weight of a detergent, 10 parts by weight of zinc dialkyl dithiophosphate, 3 parts by weight of a friction modifier, 1 part by weight of a pour point depressant, and 3 parts by weight of a neutral base oil.

[0034] In this embodiment, a method for preparing a light-load engine oil compound for improving the MRV of used oil comprises the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, then cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, then adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining 55-60°C, stirring for 2-3 hours, and filtering to obtain a light-load engine oil compound.

[0035] Example 2

[0036] In this embodiment, a light-load engine oil compound for improving the MRV of used oil includes: 65 parts by weight of a dispersant, 12 parts by weight of an antioxidant, 10 parts by weight of a detergent, 8 parts by weight of zinc dialkyl dithiophosphate, 1 part by weight of a friction modifier, 2 parts by weight of a pour point depressant, and 1 part by weight of a neutral base oil.

[0037] In this embodiment, a method for preparing a light-load engine oil compound for improving the MRV of used oil comprises the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, then cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, then adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining 55-60°C, stirring for 2-3 hours, and filtering to obtain a light-load engine oil compound.

[0038] Example 3

[0039] In this embodiment, a light-load engine oil compound for improving the MRV of used oil includes: 50 parts by weight of a dispersant, 13 parts by weight of an antioxidant, 14 parts by weight of a detergent, 15 parts by weight of zinc dialkyl dithiophosphate, 5 parts by weight of a friction modifier, 1 part by weight of a pour point depressant, and 2 parts by weight of a neutral base oil.

[0040] In this embodiment, a method for preparing a light-load engine oil compound for improving the MRV of used oil comprises the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, then cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, then adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining 55-60°C, stirring for 2-3 hours, and filtering to obtain a light-load engine oil compound.

[0041] Example 4

[0042] In this embodiment, a light-load engine oil compound for improving the MRV of used oil includes: 42 parts by weight of a dispersant, 20 parts by weight of an antioxidant, 16 parts by weight of a detergent, 12 parts by weight of zinc dialkyl dithiophosphate, 1 part by weight of a friction modifier, 4 parts by weight of a pour point depressant, and 5 parts by weight of a neutral base oil.

[0043] In this embodiment, a method for preparing a light-load engine oil compound for improving the MRV of used oil comprises the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, then cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, then adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining 55-60°C, stirring for 2-3 hours, and filtering to obtain a light-load engine oil compound.

[0044] Example 5

[0045] In this embodiment, a light-load engine oil compound for improving the MRV of used oil includes: 60 parts by weight of a dispersant, 15 parts by weight of an antioxidant, 11 parts by weight of a detergent, 9 parts by weight of zinc dialkyl dithiophosphate, 2 parts by weight of a friction modifier, 2 parts by weight of a pour point depressant, and 1 part by weight of a neutral base oil.

[0046] In this embodiment, a method for preparing a light-load engine oil compound for improving the MRV of used oil comprises the following steps: adding a dispersant and a detergent into a container, controlling the temperature to 85-90°C and mixing and stirring, then cooling to 70-75°C, adding an antioxidant and mixing and stirring, then cooling to 55-60°C, adding zinc dithiophosphate and mixing and stirring, then adding a friction modifier, a pour point depressant and a neutral base oil in sequence, maintaining 55-60°C, stirring for 2-3 hours, and filtering to obtain a light-load engine oil compound.

[0047] Comparative Example 1

[0048] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of phosphorus and sulfur, 4.5 parts by weight of di-secondary alkyl zinc salt of phosphorus and sulfur, 2 parts by weight of an oleylamine and ethylene oxide polymer, and 1 part by weight of a neutral base oil.

[0049] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that the methacrylate higher alcohol ester copolymer is deleted.

[0050] Comparative Example 2

[0051] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of phosphorus sulfate, 4.5 parts by weight of di-secondary alkyl zinc salt of phosphorus sulfate, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a fumarate ester and 1 part by weight of a neutral base oil.

[0052] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of pour point depressant is used.

[0053] Comparative Example 3

[0054] In this comparative example, a light-load engine oil compound for improving the MRV of used oil includes: 60 parts by weight of boronated polyisobutylene diimide, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of phenolic ester antioxidant, 5 parts by weight of sulfurized alkyl phenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc sulfate, 4.5 parts by weight of di-secondary alkyl zinc sulfate, 2 parts by weight of oleylamine and ethylene oxide polymer, 2 parts by weight of methacrylate high carbon alcohol ester copolymer and 1 part by weight of neutral base oil.

[0055] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of dispersant is used.

[0056] Comparative Example 4

[0057] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 60 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of sulfur and phosphorus, 4.5 parts by weight of di-secondary alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0058] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of dispersant is used.

[0059] Comparative Example 5

[0060] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 60 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of sulfur and phosphorus, 4.5 parts by weight of di-secondary alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0061] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of dispersant is used.

[0062] Comparative Example 6

[0063] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 11 parts by weight of magnesium alkyl salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of phosphorus sulfate, 4.5 parts by weight of di-secondary alkyl zinc salt of phosphorus sulfate, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0064] The preparation method of this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of detergent is used.

[0065] Comparative Example 7

[0066] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 11 parts by weight of sulfided alkyl phenol calcium, 4.5 parts by weight of dioctyl primary alkyl zinc salt of sulfur and phosphorus, 4.5 parts by weight of di-secondary alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0067] The preparation method of this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of detergent is used.

[0068] Comparative Example 8

[0069] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 9 parts by weight of dioctyl alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0070] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that different types of zinc dialkyl dithiophosphates are used.

[0071] Comparative Example 9

[0072] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 9 parts by weight of di-secondary alkyl zinc sulfate, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high-carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0073] The preparation method involved in this comparative example is the same as that of Example 5, and the main difference from Example 5 is that different types of zinc dialkyl dithiophosphates are used.

[0074] Comparative Example 10

[0075] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 15 parts by weight of nonyl diphenylamine, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of phosphorus and sulfur, 4.5 parts by weight of di-secondary alkyl zinc salt of phosphorus and sulfur, 2 parts by weight of oleylamine and ethylene oxide polymer, 2 parts by weight of methacrylate high carbon alcohol ester copolymer and 1 part by weight of neutral base oil.

[0076] The preparation method of this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of antioxidant is used.

[0077] Comparative Example 11

[0078] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 15 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of sulfur and phosphorus, 4.5 parts by weight of di-secondary alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of an oleylamine and ethylene oxide polymer, 2 parts by weight of a methacrylate high carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0079] The preparation method of this comparative example is the same as that of Example 5, and the main difference from Example 5 is that a different type of antioxidant is used.

[0080] Comparative Example 12

[0081] In this comparative example, a light-load engine oil compound for improving the MRV of used oil comprises: 8 parts by weight of boronated polyisobutylene diimide, 42 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, 10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine, 7 parts by weight of nonyl diphenylamine, 8 parts by weight of a phenolic ester antioxidant, 5 parts by weight of sulfided alkylphenol calcium, 6 parts by weight of alkyl magnesium salicylate, 4.5 parts by weight of dioctyl primary alkyl zinc salt of sulfur and phosphorus, 4.5 parts by weight of di-secondary alkyl zinc salt of sulfur and phosphorus, 2 parts by weight of a methacrylate high-carbon alcohol ester copolymer, and 1 part by weight of a neutral base oil.

[0082] The preparation method of this comparative example is the same as that of Example 5, and the main difference from Example 5 is that the friction modifier is deleted.

[0083] In summary, the component configurations of each embodiment and each comparative example are described in the form of the following table.

[0084] Table 1 Component configuration table of Examples 1-5

[0085]

[0086] Table 2 Component configuration table of Example 5 and Comparative Examples 1-12

[0087]

[0088]

[0089] Performance test: The above examples and comparative examples were respectively prepared with the same dosage (10%) into 0W-20 grade gasoline engine oil for performance evaluation.

[0090] The finished oil was prepared by referring to Table 3 below using Examples 1-5 and Comparative Examples 1-12.

[0091] Table 3 Component configuration table of finished oil prepared by using Examples 1-5 and Comparative Examples 1-12

[0092] Components 0W-20 Compound 10% Category III 100N 84.60% Adhesive agent LZ7077 6.50%

[0093] Comparative test 1: The samples were subjected to MRV test according to NB / SH / T 0562-low temperature pumping viscosity test method. Meanwhile, the new oil was aged according to CEC L-105 (biodiesel oxidation method, the test condition is to age the oil sample at 180°C for 72h in the presence of biodiesel and catalyst). The aged old oil was subjected to MRV test (at the same test temperature as the new oil). The test results are shown in Table 4 below.

[0094] Table 4 MRV determination results of different samples

[0095]

[0096] As can be seen from Table 4, after the pour point depressant was removed in Comparative Example 1, the MRV data was higher, and both the new oil and the old oil showed yield stress. After the methacrylate copolymer was replaced with fumarate in Comparative Example 2, the MRV data increased, and the effect was poor, indicating that the methacrylate copolymer and other single agents in the present invention have the best compatibility effect when they are in a certain proportion, and can provide the most excellent low-temperature pumping viscosity for engine oil.

[0097] Comparative test 2: According to NB / SH / T 0834-Determination of moderately high temperature piston deposits in engine oils by thermal oxidation simulation test method, the test temperature is 285°C, and the high temperature oxidation detergency of the test samples is tested. The test results are shown in Table 5 below.

[0098] Table 5 Test results of high temperature oxidation cleaning performance of different samples

[0099] Sample name MHT, sediment weight, mg Example 1 27.2 Example 2 40.6 Example 3 35.6 Example 4 28.2 Example 5 15.1 Comparative Example 1 17.2 Comparative Example 2 17.5 Comparative Example 3 29.3 Comparative Example 4 33.2 Comparative Example 5 35.2 Comparative Example 6 25.2 Comparative Example 7 26.5 Comparative Example 8 18.9 Comparative Example 9 21.6 Comparative Example 10 19.8 Comparative Example 11 22.6 Comparative Example 12 21.5

[0100] It should be understood that the smaller the weight of the sediment, the better the anti-oxidation and detergency of the oil. As shown in Table 5, in Comparative Examples 3, 4 and 5, one dispersant was used, and the detergency was poor. After the three were compounded in a certain ratio, the detergency was significantly improved, indicating that the three dispersants had a strong synergistic detergency effect; in Comparative Examples 6 and 7, one detergent was used, and the detergency was also poor. After the two were compounded, the detergency was good, indicating that there was also a certain synergistic effect between the two detergents.

[0101] Comparative test 3: According to SH / T 0719-Determination of oxidation induction period of lubricating oil (pressure differential scanning calorimetry - PDSC), the test temperature is 210°C, and the oxidation induction period of the test sample is tested. The test results are shown in Table 6 below.

[0102] Table 6 Test results of oxidation induction period of different samples

[0103] Sample name PDSC, min Example 1 32 Example 2 20.1 Example 3 19.6 Example 4 28.9 Example 5 39.2 Comparative Example 1 37.2 Comparative Example 2 37.5 Comparative Example 3 36.8 Comparative Example 4 37.2 Comparative Example 5 36.5 Comparative Example 6 35.2 Comparative Example 7 36.1 Comparative Example 8 25.5 Comparative Example 9 23.2 Comparative Example 10 28.4 Comparative Example 11 27.6 Comparative Example 12 34.6

[0104] It should be understood that the longer the oxidation induction period, the better the antioxidant property of the oil. As shown in Table 6, in Comparative Examples 8 and 9, a zinc dialkyl dithiophosphate was used, and the PDSC data was poor. After the two were compounded in a certain ratio, the antioxidant property was significantly improved, indicating that there was good synergistic antioxidant between the two; in Comparative Examples 10 and 11, a high-temperature antioxidant was used, and the PDSC data was also poor. After the two were compounded, the PDSC was also significantly improved, indicating that they also had good synergistic antioxidant effects.

[0105] Comparative test 4: According to SH / T 0189-Lubricating oil anti-wear performance determination method (four-ball machine method), the anti-wear and friction reduction properties of the samples were evaluated (experimental conditions: 392N, 75℃, 1200r / min, 60min). The experimental results are the wear spot diameter. The test results are shown in Table 7 below.

[0106] Table 7 Test results of wear spot diameter of different samples

[0107] Sample name Wear spot diameter, mm Example 1 0.389 Example 2 0.412 Example 3 0.369 Example 4 0.382 Example 5 0.327 Comparative Example 1 0.365 Comparative Example 2 0.362 Comparative Example 3 0.382 Comparative Example 4 0.379 Comparative Example 5 0.385 Comparative Example 6 0.378 Comparative Example 7 0.365 Comparative Example 8 0.458 Comparative Example 9 0.397 Comparative Example 10 0.37 Comparative Example 11 0.372 Comparative Example 12 0.476

[0108] It should be understood that the smaller the wear spot diameter, the better the anti-wear property of the oil. As shown in Table 7, in Comparative Examples 8 and 9, ZDDP is used, and the anti-wear property is very poor, and the two show excellent anti-wear property in a certain ratio; in Comparative Example 12, oleylamine and ethylene oxide polymer are deleted, and the anti-wear property is the worst, indicating that they play a vital role in the anti-wear of the light-load engine oil composition.

[0109] Comparative test 5: Use the MTM instrument (micro traction friction tester, no test standard yet) to evaluate the friction reduction properties of the oil. The test temperature is 120°C, the time is 2h, the friction method is the friction between the test ball and the test disc, and the traction coefficient of the test sample is tested. The test results are shown in Table 8 below.

[0110] Table 8 Test results of traction coefficient of different samples

[0111]

[0112]

[0113] It should be understood that the smaller the average traction coefficient, the better the friction reduction effect of the oil. As shown in Table 8, the friction reduction property of Comparative Example 12 is the worst when oleylamine and ethylene oxide polymer are deleted, indicating that they play a vital role in friction reduction in the light-load engine oil composition.

[0114] The above contents are further detailed descriptions of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A light-load engine oil compound for improving the MRV of used oil, characterized in that: include: 35-65 parts by weight of a dispersant, 1-20 parts by weight of a detergent, 8-15 parts by weight of zinc dialkyl dithiophosphate, 13-28 parts by weight of an antioxidant, 1-5 parts by weight of a friction modifier, 1-4 parts by weight of a pour point depressant, and 0.5-5 parts by weight of a neutral base oil. The dispersant is 7-10 parts by weight of boronated polyisobutylene succinimide, 20-45 parts by weight of a reaction product A of polyisobutylene succinic anhydride and polyene polyamine, and 7-10 parts by weight of a reaction product B of polyisobutylene succinic anhydride and polyene polyamine.

2. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The boron content in the boronated polyisobutylene succinimide is ≤0.35%, and the nitrogen content in the boronated polyisobutylene succinimide is 1.1-1.4%.

3. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The detergent comprises 6-8 parts by weight of magnesium alkyl salicylate and 4-12 parts by weight of calcium sulfide alkyl phenate.

4. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The dialkyl zinc dithiophosphate is 3-7 parts by weight of bis-octyl zinc sulfide and 4-8 parts by weight of di-secondary zinc sulfide. The zinc content of the bis-octyl zinc sulfide is 8.5-10.5%, and the zinc content of the di-secondary zinc sulfide is 7.3-8.7%.

5. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The antioxidant comprises 5-14 parts by weight of nonyl diphenylamine and 6-14 parts by weight of a phenolic ester antioxidant, wherein the nitrogen content of the nonyl diphenylamine is 3.2-3.8%.

6. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The friction modifier is oleylamine and ethylene oxide polymer, and the nitrogen content of the oleylamine and ethylene oxide polymer is 3.5-4.5%.

7. The light-duty engine oil compound for improving the MRV of used oil according to claim 1, characterized in that: The pour point depressant is a methacrylate higher alcohol ester copolymer.

8. A method for preparing a light-duty engine oil compound for improving the MRV of used oil as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: Add dispersant and detergent into the container, mix and stir at the first preset temperature, then add antioxidant and mix and stir at the second preset temperature, then add zinc dialkyl dithiophosphate and mix and stir at the third preset temperature, then add friction modifier, pour point depressant and neutral base oil in sequence, maintain the third preset temperature, stir for 2-3 hours, and obtain the light-load engine oil compound by filtering.

9. The method for preparing the light-duty engine oil compound for improving the MRV of used oil according to claim 8, characterized in that: The first preset temperature is 85-90°C, the second preset temperature is 70-75°C, and the third preset temperature is 55-60°C.

10. A light-duty engine oil compound for improving the MRV of used oil as claimed in any one of claims 1 to 7, for use in lubrication of gasoline engines and small diesel engines.

Citation Information

Patent Citations

  • Lubricating oil composition and method for improving low temperature performance of lubricating oil

    CN108003971A

  • Lubricating oil pour point depressant and preparation method thereof

    CN112079951A