Annealing process of 5A02 O-state conduit with high structure property uniformity

By using the metal mesh bottomed basket and optimizing the finished annealing process in the annealing process of 5A02 O-state aluminum alloy pipes, the problems of unevenness and fracture of the conduit are solved, and the uniformity and stability of high tissue performance are achieved, which is suitable for industrialization. Production.

CN118979144APending Publication Date: 2024-11-19SOUTHWEST ALUMINUM GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044947.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing 5A02 O-state aluminum alloy conduits have large performance fluctuations and large low-power tissue grain sizes in aircraft applications, resulting in flaring orange peel and breaking after bending. The finished product annealing process and tooling are inappropriate, resulting in material structure and Uneven performance.

Method used

The annealing process for preparing 5A02 O-state aluminum alloy tubes is adopted using a basket with a metal mesh bottom. By optimizing the composition and finished annealing process, a new finished annealing tool is designed. The high-temperature, short-term heating and fast cooling process is adopted to control the Mg content at 2.0%. ~2.5%, and optimized by specific finished product annealing tooling and process to ensure metal temperature uniformity and tissue uniformity.

Benefits of technology

The production of 5A02 O-state catheter with high tissue uniformity reduces the risk of orange peel defects and bending after bending, meets higher application needs, and is simple in process and good controllability, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977497400000061
    Figure BDA0004977497400000061
  • Figure BDA0004977497400000071
    Figure BDA0004977497400000071
  • Figure BDA0004977497400000081
    Figure BDA0004977497400000081
Patent Text Reader

Abstract

The invention provides application of a charging basket with a metal net bottom in preparation of a 5A02O-state aluminum alloy pipe. The invention also provides an annealing process of the 5A02O state conduit with high structure property uniformity. By means of 5A02 alloy component optimization, reasonable design of a finished product annealing tool, optimization of guide pipe finished product annealing operation requirements and the like, after the specific finished product annealing tool is combined with the 5A02 (LF2M) aluminum pipe annealing process optimization, the temperature uniformity of metal materials of different specifications and different charge quantities is obviously improved compared with the temperature uniformity before optimization. Alloy components are optimized, the strength of the material is reduced, bending and flaring deformation of the material are facilitated, meanwhile, a finished product annealing process and a finished product annealing tool are optimized, the annealing temperature uniformity of the material and the uniformity of the structure are improved, and the yield is increased. Therefore, the 5A02 O-state guide pipe which meets higher requirements of follow-up manufacturers and is high in structure performance uniformity can be produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of 5A02 O-state aluminum alloy tube preparation, relates to the application of a material basket with a metal mesh bottom in the preparation of a 5A02 O-state aluminum alloy tube and an annealing process for the 5A02 O-state aluminum alloy tube, and in particular to an annealing process for a 5A02 O-state conduit with high uniformity of organizational properties. Background Art

[0002] 5A02 O-state thin-walled pipes are used for fuel, hydraulic and environmental control system pipes in aircraft. In order to further meet the needs of the new generation of aviation equipment, downstream application manufacturers have put forward higher requirements for the performance and organization of pipes, which are far higher than the requirements of the current national standard GB / T6893-2022. Moreover, due to the constraints of domestic equipment and preparation technology, the pipes currently produced have problems such as large performance fluctuations and large low-multiple grain size. The supply of key materials has "bottleneck" problems such as quality and delivery time. At the same time, internationally, companies such as Arconic, UAC, KAISER in the United States, Una in Germany, and Hydro in Sweden provide professional and high-quality small pipes to aviation companies around the world, forming a strong competition.

[0003] At present, the domestic process flow for producing 5A02O-state catheters is basically the same, but the performance fluctuates greatly and the grain size of the low-magnification structure is large, which leads to problems such as orange peel at the mouth expansion and breakage after bending during use by downstream application manufacturers.

[0004] Therefore, how to find a more suitable processing technology to solve the above-mentioned problems existing in the existing 5A02 O-state aluminum alloy conduits has become one of the urgent issues to be solved by many front-line researchers in the industry. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide an application of a material basket with a metal mesh bottom in the preparation of a 5A02O-state aluminum alloy tube and an annealing process for a 5A02O-state aluminum alloy tube, in particular, an annealing process for a 5A02O-state conduit with high uniformity of organizational properties. The present invention optimizes the 5A02 composition and the finished product annealing process and designs a new finished product annealing tooling, thereby being able to produce a 5A02O-state conduit with high uniformity of organizational properties that meets the higher requirements of subsequent manufacturers. At the same time, the annealing process provided by the present invention is simple, has good controllability, simple tooling, good operability, and is more suitable for the promotion and application of industrial production.

[0006] The invention provides application of a material basket with a metal mesh bottom in preparing a 5A02 O-state aluminum alloy tube.

[0007] Preferably, the preparation is specifically an annealing process for preparing a 5A02 O-state aluminum alloy tube;

[0008] The metal mesh comprises a high temperature resistant metal mesh;

[0009] The heat-resistant metal mesh has a heat-resistant temperature of 800-850°C.

[0010] Preferably, the aluminum alloy tube comprises an aluminum alloy conduit;

[0011] The diameter of the 5A02 O-state aluminum alloy tube is φ6-φ85 mm;

[0012] The wall thickness of the 5A02 O-state aluminum alloy tube is 1-2 mm.

[0013] Preferably, the material basket is specifically a material basket placed in an annealing furnace during the annealing process;

[0014] The metal mesh bottom is specifically a metal mesh bottom for placing the 5A02 O-state aluminum alloy tube in annealing;

[0015] The mesh size of the metal mesh bottom is 30mm*30mm.

[0016] Preferably, the metal mesh bottom comprises a single-layer metal mesh bottom or a multi-layer metal mesh bottom;

[0017] A single-layer 5A02 O-state aluminum alloy tube and / or a multi-layer 5A02 O-state aluminum alloy tube are placed on the single-layer metal mesh bottom;

[0018] A single-layer 5A02 O-state aluminum alloy tube is placed at the bottom of the multi-layer metal mesh;

[0019] The number of the multi-layers is 2 to 5.

[0020] Preferably, the application includes reducing orange peel defects on the expanded end face of the aluminum alloy tube, reducing cracking of the expanded aluminum alloy tube, and reducing cracking of the aluminum alloy tube after flattening;

[0021] In the 5A02 O-state aluminum alloy tube, the Mg content is 2.0% to 2.5% by mass.

[0022] The present invention provides an annealing process for a 5A02 O-state aluminum alloy tube, comprising the following steps:

[0023] 1) After the annealing furnace is baked, the 5A02 aluminum alloy tube is loaded into a basket with a metal mesh bottom, and then placed in the annealing furnace for annealing treatment to obtain a 5A02 O-state aluminum alloy tube;

[0024] The 5A02 aluminum alloy tube comprises, by mass percentage, Mg: 2.0% to 2.5%, Mn and / or Cr: 0.15% to 0.40%, Fe≤0.40%, Si≤0.40%, Cu≤0.10%, Ti≤0.15%, and the remainder Al and impurity elements; wherein the content of Fe+Si is ≤0.6%.

[0025] Preferably, the temperature of the baking oven is 470-490°C;

[0026] The baking time is greater than or equal to 45 minutes;

[0027] In the 5A02 aluminum alloy tube, the mass content of a single impurity is ≤0.05%, and the total mass content of impurities is ≤0.15%.

[0028] Preferably, the material basket is placed on a material cart and placed in an annealing furnace for annealing;

[0029] The material basket is placed in front of the annealing furnace, and the temperature of the material basket near the furnace door is less than or equal to 80°C;

[0030] Single-layer and / or multi-layer baskets are stacked in a single row or multiple rows on the material cart;

[0031] The multi-layers include 2 to 5 layers.

[0032] Preferably, the annealing temperature is 400-455°C;

[0033] The annealing time is 10 min;

[0034] During the annealing process, the temperature difference of the 5A02 aluminum alloy tube is less than or equal to 30°C.

[0035] The present invention provides the use of a material basket with a metal mesh bottom in the preparation of 5A02 O-state aluminum alloy tubes. Compared with the prior art, the present invention believes that the problems of orange peel at the expanded mouth and fracture after bending in the subsequent application of 5A02 O-state aluminum alloy tubes are mainly caused by the large grain size of the material's macrostructure and the high and uneven tensile strength. The root cause is mainly the unreasonable component design. The main element of 5A02 alloy is Mg. In order to improve the strength of the material, the Mg content is relatively high, and its mass fraction is 2.5-2.8%. However, the excessive strength will cause the expanded end surface to be orange peel or even cracked during the expansion process, and greatly reduce the strength of the expanded part. Figure 1As shown in the figure, in the subsequent harsh use environment, it is easy to cause oil leakage at the flared connection; and the finished product annealing process and tooling are not properly matched. During the finished product annealing, in order to reduce the tensile strength of the material and change the cold-processed pipe structure from a fibrous state to a fully recrystallized structure. The production process of "high temperature, short-time heating, and rapid cooling" can obtain a fine grain size, but due to the influence of annealing tooling design, furnace loading, and rapid cooling method, the organization and performance of the material are extremely unstable, resulting in continuous quality problems of the subsequent pipes.

[0036] Based on this, the present invention specially designs a finished product annealing tool with a specific structure for the annealing process of 5A02 O-state aluminum alloy tube. Furthermore, the present invention also optimizes the 5A02 composition and finished product annealing process, so as to produce 5A02 O-state tubes with high uniformity of organizational performance that meet the higher requirements of subsequent manufacturers. At the same time, the annealing process provided by the present invention is simple, has good controllability, simple tooling, good operability, and is more suitable for the promotion and application of industrial production.

[0037] The present invention optimizes the 5A02 composition, and Mg mainly exists in the solid solution state and (Mg2 A12 or Mg, Alg) phase. Although the solubility of Mg in the alloy decreases rapidly with decreasing temperature, the alloy has low aging strengthening effect due to the difficulty of precipitation nucleation, small number of cores, and coarse precipitation phases. It is generally used in annealing or cold working state. The strength of this series of alloys increases with the increase of Mg content, while the plasticity decreases accordingly, and its processing performance also deteriorates accordingly. Therefore, the present invention controls the Mg content at a lower limit of 2.0% to 2.5%.

[0038] The present invention solves the above technical problems by optimizing the 5A02 alloy composition, reasonably designing the finished product annealing tooling, optimizing the finished product annealing operation requirements of the conduit, etc. The present invention adopts a specific finished product annealing tooling combined with the 5A02 (LF2M) aluminum tube annealing process optimization, and the uniformity of metal material temperature of different specifications and different furnace loading amounts is significantly improved compared with before optimization; according to the test results comparing the limit furnace loading basket number, the actual metal temperature reaches above 310°C, the recrystallization is sufficient, and different furnace loading basket numbers are suitable for the production of LF2M aluminum tubes.

[0039] The invention optimizes the alloy composition and reduces the strength of the material, which is beneficial to the bending and expansion deformation of the material. At the same time, it optimizes the finished product annealing process and finished product annealing tooling, and improves the annealing temperature uniformity and organizational uniformity of the material.

[0040] The experimental results show that 100% of the samples were taken at different temperature measurement points to test the mechanical properties, flattening and grain size of typical specifications. The tensile strength was qualified, the tensile strength Cv value of each specification was less than 3%, the elongation was ≥15%, there was no cracking after flattening, and the grain size was ≤1 level. After re-testing and process verification tests such as bending and flaring, the results were all qualified. The LF2M aluminum tube produced by the present invention using the optimized finished product annealing process meets the requirements of the GJB2379A standard in all technical indicators, and has good uniformity and consistency. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The photos of orange peel and cracking on the expanded end surface of the existing 5A02 O-state aluminum alloy tube;

[0042] Figure 2 A schematic structural diagram of the annealing furnace hearth used in the present invention;

[0043] Figure 3 Appearance of the annealing basket that serves as the base for the existing aluminum square tube;

[0044] Figure 4 This is the appearance diagram of the annealing basket of the aluminum mesh plate and the stainless steel mesh used in the present invention;

[0045] Figure 5 Schematic diagram of the change of the basket loading method before and after optimization; wherein the left figure is the existing basket loading method, and the right figure is the basket loading method adopted by the present invention;

[0046] Figure 6 It is a schematic diagram showing the arrangement of material baskets with 3 baskets and 6 baskets per furnace in an embodiment of the present invention;

[0047] Figure 7 This is a graph showing the maximum temperature distribution of three baskets of aluminum tubes in an embodiment of the present invention;

[0048] Figure 8 This is a graph showing the maximum temperature distribution of 6 baskets of aluminum tubes in an embodiment of the present invention;

[0049] Fig. 9 This is a photo of the flattened sample of some existing 5A02 O-state aluminum alloy tubes at low grain size;

[0050] Fig.10 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ6×1 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0051] Fig.11 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ12×1 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0052] Fig.12 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ16×1 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0053] Fig.13 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ20×1 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0054] Fig.14 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ42×1 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0055] Fig.15 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ75×1.5 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point;

[0056] Fig.16 The high-magnification grain structure diagrams of the high-temperature point and the low-temperature point of Φ85×2.0 in the embodiment of the present invention are shown; wherein the upper figure is the high-magnification grain structure diagram of the high-temperature point, and the lower figure is the high-magnification grain structure diagram of the low-temperature point. DETAILED DESCRIPTION

[0057] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.

[0058] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0059] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses industrial pure or 5A02O aluminum alloy tubes with conventional purity requirements in the field of preparation.

[0060] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.

[0061] The abbreviations of the processes used in the present invention are all conventional abbreviations in the field. The specific steps and conventional parameters of each abbreviation are clear and definite in its relevant field. Those skilled in the art can implement them in a conventional manner based on the abbreviations.

[0062] The invention provides application of a material basket with a metal mesh bottom in preparing a 5A02 O-state aluminum alloy tube.

[0063] In the present invention, the preparation is preferably an annealing process for preparing a 5A02 O-state aluminum alloy tube.

[0064] In the present invention, the metal mesh preferably includes a high temperature resistant metal mesh.

[0065] In the present invention, the heat-resistant temperature of the high-temperature resistant metal mesh is preferably 800-850°C, more preferably 810-840°C, and more preferably 820-830°C.

[0066] In the present invention, the aluminum alloy tube preferably includes an aluminum alloy conduit.

[0067] In the present invention, the diameter of the 5A02 O-state aluminum alloy tube is preferably φ6-φ85 mm, more preferably φ20-φ70 mm, and even more preferably φ40-φ50 mm.

[0068] In the present invention, the wall thickness of the 5A02 O-state aluminum alloy tube is preferably 1-2 mm, more preferably 1.2-1.8 mm, and more preferably 1.4-1.6 mm.

[0069] In the present invention, the material basket is preferably a material basket placed in an annealing furnace during the annealing process.

[0070] In the present invention, the metal mesh bottom is preferably a metal mesh bottom on which a 5A02 O-state aluminum alloy tube undergoing annealing is placed.

[0071] In the present invention, the mesh size of the metal mesh bottom is preferably 30 mm*30 mm.

[0072] In the present invention, the metal mesh bottom preferably includes a single-layer metal mesh bottom or a multi-layer metal mesh bottom.

[0073] In the present invention, a single-layer 5A02 O-state aluminum alloy tube and / or multiple layers of 5A02 O-state aluminum alloy tubes are preferably placed on the single-layer metal mesh bottom, and a single-layer 5A02 O-state aluminum alloy tube or multiple layers of 5A02 O-state aluminum alloy tubes are more preferably placed.

[0074] In the present invention, the multi-layer metal mesh bottom is preferably provided with a single-layer 5A02 O-state aluminum alloy tube;

[0075] In the present invention, the number of the multilayer is preferably 2 to 5 layers, more preferably 3 or 4 layers.

[0076] In the present invention, the application preferably includes reducing the orange peel defect on the expanded end face of the aluminum alloy tube, reducing the cracking of the expanded aluminum alloy tube, and reducing the cracking of the aluminum alloy tube after flattening. Specifically, the application is preferably an application in avoiding the orange peel defect on the expanded end face of the aluminum alloy tube, avoiding the cracking of the expanded aluminum alloy tube, and avoiding the cracking of the aluminum alloy tube after flattening.

[0077] In the present invention, in the 5A02 O-state aluminum alloy tube, the Mg content is preferably 2.0% to 2.5% by mass, more preferably 2.1% to 2.4%, and more preferably 2.2% to 2.3% by mass.

[0078] The present invention provides an annealing process for a 5A02 O-state aluminum alloy tube, comprising the following steps:

[0079] 1) After the annealing furnace is baked, the 5A02 aluminum alloy tube is loaded into a basket with a metal mesh bottom, and then placed in the annealing furnace for annealing treatment to obtain a 5A02 O-state aluminum alloy tube.

[0080] In the present invention, the 5A02 aluminum alloy tube comprises, by mass percentage, Mg: 2.0% to 2.5%, Mn and / or Cr: 0.15% to 0.40%, Fe≤0.40%, Si≤0.40%, Cu≤0.10%, Ti≤0.15%, and the remainder of Al and impurity elements; wherein the content of Fe+Si is ≤0.6%, which may be Mg: 2.1% to 2.4%, Mn and / or Cr: 0.20% to 0.35%, Fe≤0.35%, Si≤0.35%, Cu≤0.09%, Ti≤0.13%, which may be Mg: 2.2% to 2.3%, Mn and / or Cr: 0.25% to 0.30%, Fe≤0.30%, Si≤0.30%, Cu≤0.08%, and Ti≤0.11%.

[0081] In the present invention, the temperature of the baking oven is preferably 470-490°C, more preferably 474-486°C, more preferably 478-482°C, and specifically may be 480°C.

[0082] In the present invention, the baking time is preferably greater than or equal to 45 min, more preferably greater than or equal to 46 min, and more preferably greater than or equal to 47 min.

[0083] In the present invention, in the 5A02 aluminum alloy tube, the mass content of a single impurity is preferably ≤0.05%, and the total mass content of impurities is ≤0.15%, more preferably the mass content of a single impurity is ≤0.04%, and the total mass content of impurities is ≤0.14%, more preferably the mass content of a single impurity is ≤0.03%, and the total mass content of impurities is ≤0.13%.

[0084] In the present invention, the material basket is preferably placed on a material cart and placed in an annealing furnace for annealing.

[0085] In the present invention, the basket is placed in front of the annealing furnace, and the temperature of the basket near the furnace door is preferably less than or equal to 80°C, more preferably less than or equal to 75°C, and more preferably less than or equal to 70°C.

[0086] In the present invention, the material cart preferably has single-layer and / or multi-layer material baskets stacked in a single row or multiple rows, and more preferably has single-layer or multi-layer material baskets stacked in a single row or multiple rows.

[0087] In the present invention, the multilayer preferably includes 2 to 5 layers, more preferably 3 or 4 layers.

[0088] In the present invention, the annealing temperature is preferably 400-455° C., more preferably 410-445° C., and more preferably 420-435° C. Specifically, during the annealing process, the metal temperature preferably reaches 400-455° C.

[0089] In the present invention, the annealing time is preferably 10 minutes.

[0090] In the present invention, during the annealing process, the temperature difference of the 5A02 aluminum alloy tube is preferably less than or equal to 30°C.

[0091] See Table 1, which is a comparison of the performance requirements of the 5A02 O-state aluminum alloy tube prepared by the present invention and the performance requirements of the national standard.

[0092] Table 1

[0093]

[0094] It can be seen from Table 1 that the performance of the 5A02 O-state aluminum alloy tube prepared by the present invention is much higher than the requirements of the current national standard GB / T6893-2022. The present invention can produce a 5A02 O-state aluminum alloy tube with high uniformity of structure and performance that can meet the needs of subsequent application manufacturers.

[0095] See Table 2, which shows the chemical composition requirements of the 5A02 O-state aluminum alloy tube provided by the present invention.

[0096] Table 2

[0097]

[0098] The above content of the present invention provides the use of a material basket with a metal mesh bottom in the preparation of a 5A02 O-state aluminum alloy tube and an annealing process for a 5A02 O-state conduit with high uniformity of organizational properties. The finished product annealing tooling specially designed by the present invention with a specific structure is used in the annealing process of the 5A02 O-state aluminum alloy tube. Furthermore, the present invention also optimizes the 5A02 composition and the finished product annealing process, thereby being able to produce a 5A02 O-state conduit with high uniformity of organizational properties that meets the higher requirements of subsequent manufacturers. At the same time, the annealing process provided by the present invention is simple, has good controllability, simple tooling, good operability, and is more suitable for the promotion and application of industrial production.

[0099] The present invention optimizes the 5A02 composition, and Mg mainly exists in the solid solution state and (Mg2 A12 or Mg, Alg) phase. Although the solubility of Mg in the alloy decreases rapidly with decreasing temperature, the alloy has low aging strengthening effect due to the difficulty of precipitation nucleation, small number of cores, and coarse precipitation phases. It is generally used in annealing or cold working state. The strength of this series of alloys increases with the increase of Mg content, while the plasticity decreases accordingly, and its processing performance also deteriorates accordingly. Therefore, the present invention controls the Mg content at a lower limit of 2.0% to 2.5%.

[0100] The present invention solves the above technical problems by optimizing the 5A02 alloy composition, reasonably designing the finished product annealing tooling, optimizing the finished product annealing operation requirements of the conduit, etc. The present invention adopts a specific finished product annealing tooling combined with the 5A02 (LF2M) aluminum tube annealing process optimization, and the uniformity of metal material temperature of different specifications and different furnace loading amounts is significantly improved compared with before optimization; according to the test results comparing the limit furnace loading basket number, the actual metal temperature reaches above 310°C, the recrystallization is sufficient, and different furnace loading basket numbers are suitable for the production of LF2M aluminum tubes.

[0101] The invention optimizes the alloy composition and reduces the strength of the material, which is beneficial to the bending and expansion deformation of the material. At the same time, it optimizes the finished product annealing process and finished product annealing tooling, and improves the annealing temperature uniformity and organizational uniformity of the material.

[0102] The experimental results show that 100% of the samples were taken at different temperature measurement points to test the mechanical properties, flattening and grain size of typical specifications. The tensile strength was qualified, the tensile strength Cv value of each specification was less than 3%, the elongation was ≥15%, there was no cracking after flattening, and the grain size was ≤1 level. After re-testing and process verification tests such as bending and flaring, the results were all qualified. The LF2M aluminum tube produced by the present invention using the optimized finished product annealing process meets the requirements of the GJB2379A standard in all technical indicators, and has good uniformity and consistency.

[0103] To further illustrate the present invention, the application of the material basket with a metal mesh bottom provided by the present invention in the preparation of 5A02 O-state aluminum alloy tubes and an annealing process of 5A02 O-state aluminum alloy tubes are described in detail below in combination with the embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating procedures are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following embodiments.

[0104] Example

[0105] See Table 3, which shows the chemical composition of the 5A02 O-state aluminum alloy tube provided in the embodiment of the present invention.

[0106] Table 3

[0107]

[0108] Finished product annealing process and tooling

[0109] Trial plan

[0110] When the prepared LF2M aluminum tube is annealed in the annealing furnace, the operation is carried out according to the following requirements:

[0111] Baking furnace: empty furnace set temperature 480℃, after reaching temperature, keep warm for no less than 45min;

[0112] Furnace loading: After the furnace is baked, all furnace doors are opened and the hot furnace is loaded. Before loading, ensure that the temperature of the material cart near the furnace door is below 80℃;

[0113] Annealing: After closing the furnace door, set the furnace temperature to 450℃, then start the heating button. After the furnace gas reaches the temperature, the equipment automatically starts calculating the insulation time, and the furnace is taken out after 10 minutes of insulation.

[0114] Out of the oven: After the insulation is completed, the car is taken out of the oven. After all the carts are out of the oven, turn on the axial flow fan for rapid cooling.

[0115] Basket structure

[0116] Annealing furnace structure Figure 2 After the air is heated by the resistance wires on both sides, it is drawn from the heating chamber to the furnace through the fan to heat the workpiece, and the heating cycle is repeated.

[0117] In order to prevent the aluminum tube from bending and deforming during the annealing process, the original annealing basket uses aluminum square tubes as the bottom (see Figure 3 ), since the hot air is blown in from both sides of the basket, it objectively affects the hot air circulation effect.

[0118] In order to improve the hot air circulation effect, the bottom material of the basket was designed with two structures: aluminum mesh and stainless steel mesh. However, the aluminum mesh was bent and deformed after being used once, so stainless steel mesh was used as the bottom material. At the same time, in order to increase the furnace loading capacity, a grid was added in the height direction of the basket. Figure 4 .

[0119] Basket loading method

[0120] When the aluminum tubes are loaded into the basket, in order to further improve the uniformity of the metal temperature and reduce the metal temperature difference between the aluminum tubes, a spacer is laid horizontally at intervals along the length of the stainless steel mesh. And only one layer of aluminum tubes is placed in each grid. The material basket and loading method before and after optimization are shown in the figure. Figure 5 .

[0121] Test specifications

[0122] The minimum specification of LF2M aluminum tube is φ6×1.0mm, and the maximum specification is φ85×2.0mm. In order to ensure the representativeness of the verification results, the smallest φ6×1.0mm aluminum tube and the largest φ85×2.0mm aluminum tube were selected for verification, and 5 types of intermediate specifications (φ12×1.0mm, φ16×1.0mm, φ20×1.0mm, φ42×1.0mm, φ75×1.5mm) were selected for finished product annealing effect verification. The mechanical properties, grain size and flattening of the aluminum tubes need to be tested.

[0123] See Table 4, which is a detailed list of aluminum tubes in the embodiments of the present invention.

[0124] Table 4

[0125]

[0126] The placement of the baskets for each furnace with 3 and 6 baskets is as follows Figure 6 shown.

[0127] Heat treatment data analysis

[0128] See Table 5, which is a statistical data of total heating time and metal temperature for annealing of finished products of 7 typical specifications in the embodiments of the present invention.

[0129] Table 5

[0130]

[0131] The maximum temperature distribution of three baskets of metal of each specification during annealing is shown in Figure 7 , the maximum metal temperature distribution of 6 baskets is shown in Figure 8 .

[0132] From Table 5 and Figure 7It can be seen that when single stack is used (i.e. 3 baskets are loaded), the highest metal temperature of typical specifications after leaving the furnace is between 425.49℃ and 451.3℃, and the temperature difference between the highest and lowest metal temperatures of different specifications is between 12.98℃ and 25.79℃.

[0133] From Table 5 and Figure 8 It can be seen that the maximum metal temperature during the annealing process of typical specifications placed in double stacks (i.e. when 6 baskets are loaded) is between 432.0℃ and 454.9℃, and the temperature difference between the maximum and minimum metal temperatures of different specifications is between 11.3℃ and 21.3℃.

[0134] Effect of different number of furnace baskets of the same specification on metal temperature

[0135] During the period, the influence of different number of furnace baskets of the same specification on the metal temperature of aluminum tubes was tested, and the heat treatment differences of 3 and 6 baskets of φ42×1.0mm specification, 1 and 3 baskets of φ12×1.0mm specification, and 1 and 6 baskets of φ75×1.5mm specification were compared. The relevant data are shown in Table 6. Table 6 is the annealing data of aluminum tubes with different furnace loading amounts in the embodiment of the present invention.

[0136] Table 6

[0137]

[0138] The test results show that as the number of furnace baskets increases, the total heating time for aluminum tube annealing increases; the metal temperature of aluminum tubes of different specifications and different furnace loadings all reaches above 310°C before leaving the furnace; the metal temperature difference at typical positions of aluminum tubes with different furnace loadings is less than 30°C.

[0139] Test results

[0140] Sampling requirements

[0141] After the temperature measurement of 7 typical specifications was completed, Southwest Aluminum tested the room temperature tensile properties, low-magnification grain size and flattening properties, and sampled at the corresponding position of the pipe temperature measurement point. The sampling requirements for each test item were implemented according to Table 7. Table 7 is the sampling rules for the test items in the embodiment of the present invention.

[0142] Table 7

[0143]

[0144] Test results

[0145] According to the requirements of GJB2379A standard, the room temperature mechanical properties, low-magnification grain size and flattening performance tests are carried out. The test results are shown in Tables 8 to 14. The index requirements are as follows: the low-magnification grain size level is not allowed to exceed level 1, the tensile strength is 167 to 225 MPa, the elongation is ≥15%, and the flattening is performed until the middle of the inner wall of the tube contacts without cracking.

[0146] Table 8 Room temperature mechanical properties

[0147]

[0148] Table 9 Room temperature mechanical properties

[0149]

[0150]

[0151] Table 10 Room temperature mechanical properties

[0152]

[0153] Table 11 Room temperature mechanical properties

[0154]

[0155] Table 12 Room temperature mechanical properties

[0156]

[0157]

[0158] Table 13 Room temperature mechanical properties

[0159]

[0160]

[0161] Table 14 Room temperature mechanical properties

[0162]

[0163]

[0164] Data analysis was performed on the tensile strength of 7 typical specifications, and the CV value of the tensile strength of each typical specification was <3.0%, as shown in Table 15. Referring to Table 15, Table 15 is a statistical data of mechanical properties in the embodiments of the present invention.

[0165] Table 15

[0166]

[0167]

[0168] The low-magnification grain size and flattening results of the existing 5A02 O-state aluminum alloy tube typical specifications are shown in Fig. 9 .

[0169] The high-magnification grain structure of each specification at the highest temperature point and the lowest temperature point in the embodiment of the present invention was detected. Figure 10 to Figure 16 , Figure 10 to Figure 16 The high-magnification grain structures of the pipes of various specifications prepared in the embodiments of the present invention are shown in FIG.

[0170] like Fig.10 As shown, the average grain size at the high temperature point is 29.6 μm, and the average grain size at the low temperature point is 20.16 μm.

[0171] like Fig.11 As shown, the average grain size at the high temperature point is 29.6 μm, and the average grain size at the low temperature point is 20.16 μm.

[0172] like Fig.12 As shown, the average grain size at the high temperature point is 38.21 μm, and the average grain size at the low temperature point is 34.12 μm.

[0173] like Fig.13 As shown, the average grain size at the high temperature point is 31.22 μm, and the average grain size at the low temperature point is 33.64 μm.

[0174] like Fig.14 As shown, the average grain size at the high temperature point is 30.55 μm, and the average grain size at the low temperature point is 32.62 μm.

[0175] like Fig.15 As shown, the average grain size at the high temperature point is 47.32 μm, and the average grain size at the low temperature point is 44.62 μm.

[0176] like Fig.16 As shown, the average grain size at the high temperature point is 53.31 μm, and the average grain size at the low temperature point is 56.2 μm.

[0177] The performance and organizational results of the LF2M aluminum tube after annealing of the finished product show that the performance uniformity of the production is good after the annealing process is optimized, and the recrystallization of the aluminum tube fully meets the requirements of the GJB2379A standard.

[0178] Comparison before and after optimization process

[0179] Process comparison

[0180] The comparison of the finished product annealing process before and after optimization is shown in Table 16. Table 16 is the comparison data of the finished product annealing process of the present invention and the existing one.

[0181] Table 16

[0182] project Before optimization After optimization Basket length 4.5 m 4.5 m Basket bottom material Aluminum square tube Stainless Steel Mesh Aluminum tube basket loading method Aluminum tube multilayer stacking Each basket has two compartments, one compartment per layer

[0183] Results comparison

[0184] At the same time, the relevant data before and after the annealing process optimization are compared, as shown in Table 17. Table 17 is a comparison of the relevant data before and after the optimization of the finished product annealing process of the present invention and the existing one.

[0185] Table 17

[0186]

[0187] The above is a detailed introduction to the application of the material basket with a metal mesh bottom provided by the present invention in the preparation of 5A02 O-state aluminum alloy tubes and an annealing process of a 5A02 O-state catheter with high uniformity of organizational properties. The principles and implementation methods of the present invention are described in detail using specific examples. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the textual expression of the claims, or if they include equivalent structural elements that are not substantially different from the textual expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. Application of a basket with a metal mesh bottom in the preparation of 5A02 O-state aluminum alloy tubes.

2. The use according to claim 1, characterized in that: The preparation is specifically an annealing process for preparing a 5A02O aluminum alloy tube; The metal mesh comprises a high temperature resistant metal mesh; The heat-resistant metal mesh has a heat-resistant temperature of 800-850°C.

3. The use according to claim 2, characterized in that: The aluminum alloy tube comprises an aluminum alloy conduit; The diameter of the 5A02 O-state aluminum alloy tube is φ6-φ85 mm; The wall thickness of the 5A02 O-state aluminum alloy tube is 1-2 mm.

4. The use according to claim 2, characterized in that: The material basket is specifically a material basket placed in an annealing furnace during the annealing process; The metal mesh bottom is specifically a metal mesh bottom for placing the 5A02 O-state aluminum alloy tube in annealing; The mesh size of the metal mesh bottom is 30mm*30mm.

5. The use according to claim 4, characterized in that: The metal mesh bottom includes a single-layer metal mesh bottom or a multi-layer metal mesh bottom; A single-layer 5A02 O-state aluminum alloy tube and / or a multi-layer 5A02 O-state aluminum alloy tube are placed on the single-layer metal mesh bottom; A single-layer 5A02 O-state aluminum alloy tube is placed at the bottom of the multi-layer metal mesh; The number of the multi-layers is 2 to 5.

6. The use according to claim 1, characterized in that: The applications include reducing orange peel defects on the expanded end face of aluminum alloy tubes, reducing cracking of expanded aluminum alloy tubes, and reducing cracking of aluminum alloy tubes after flattening; In the 5A02 O-state aluminum alloy tube, the Mg content is 2.0% to 2.5% by mass.

7. An annealing process for a 5A02 O-state aluminum alloy tube, characterized in that: The following steps are involved: 1) After the annealing furnace is baked, the 5A02 aluminum alloy tube is loaded into a basket with a metal mesh bottom, and then placed in the annealing furnace for annealing treatment to obtain a 5A02 O-state aluminum alloy tube; The 5A02 aluminum alloy tube comprises, by mass percentage, Mg: 2.0% to 2.5%, Mn and / or Cr: 0.15% to 0.40%, Fe≤0.40%, Si≤0.40%, Cu≤0.10%, Ti≤0.15%, and the remainder Al and impurity elements; wherein the content of Fe+Si is ≤0.6%.

8. The annealing process according to claim 7, characterized in that: The temperature of the baking oven is 470-490°C; The baking time is greater than or equal to 45 minutes; In the 5A02 aluminum alloy tube, the mass content of a single impurity is ≤0.05%, and the total mass content of impurities is ≤0.15%.

9. The annealing process according to claim 7, characterized in that: The material basket is specifically placed on a material cart and placed in an annealing furnace for annealing; The material basket is placed in front of the annealing furnace, and the temperature of the material basket near the furnace door is less than or equal to 80°C; Single-layer and / or multi-layer baskets are stacked in a single row or multiple rows on the material cart; The multi-layers include 2 to 5 layers.

10. The annealing process according to claim 7, characterized in that: The annealing temperature is 400-455°C; The annealing time is 10 min; During the annealing process, the temperature difference of the 5A02 aluminum alloy tube is less than or equal to 30°C.