High-bending-property 1300MPa-grade cold-rolled martensitic steel and preparation method thereof

Through continuous annealing process optimization, the bending performance of 1300MPa grade cold-rolled martensite steel is improved, and the problem of insufficient bending performance of martensite steel in the existing technology is solved, and high strength and excellent bending performance is achieved. It is suitable for the automotive industry lightweight and reduce energy consumption requirements.

CN119061242AActive Publication Date: 2024-12-03SHOUGANG GROUP CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411240483.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

How to improve the bending performance of 1300MPa grade cold-rolled martensitic steel to meet the automotive industry's demand for high-strength and lightweight materials.

Method used

By the preparation method, the method includes continuously annealing of the cold hard plate with a set chemical composition, the specific steps include first heating to a first temperature for pre-oxidation and insulation, second heating to a second temperature for slow cooling and fast cooling, and The third temperature is over-ageable to optimize the structural structure and mechanical properties of martensite steel.

Benefits of technology

The preparation of cold-rolled martensite steel with high bending performance of 1300MPa grade is achieved, with tensile strength >1300MPa, yield strength 1030MPa~1300MPa, elongation A80≥3%, and satisfies the 180° bending performance parallel to the rolling direction without cracking The microstructure includes 92% to 96% of slat martensite and 4% to 8% of ferrite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061242A_ABST
    Figure CN119061242A_ABST
Patent Text Reader

Abstract

The invention relates to high-bending-property 1300MPa-grade cold-rolled martensitic steel and a preparation method thereof. The method comprises the following steps: obtaining a chilled plate with set chemical components; the cold-hardened plate is subjected to continuous annealing, and the high-bending-property 1300MPa-grade cold-rolled martensitic steel is obtained, specifically, the cold-hardened plate is subjected to first heating to a first temperature, the surface layer of the cold-hardened plate with the first temperature is pre-oxidized under the condition of a first dew point, first heat preservation is conducted under the condition of the first temperature, and a first annealed plate is obtained; carrying out second heating on the first annealed plate to a second temperature, carrying out second heat preservation under the condition of the second temperature, and then carrying out slow cooling and rapid cooling to obtain a second annealed plate; and the second annealed plate is subjected to third heating to a third temperature, overaging is carried out under the condition of first set time, and the high-bending-property 1300MPa-grade cold-rolled martensitic steel is obtained. The bending property of the 1300MPa-grade cold-rolled martensitic steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel preparation, and in particular to a high-bending-performance 1300MPa-grade cold-rolled martensitic steel and a preparation method thereof. Background Art

[0002] With the rapid development of the global automotive industry, lightweighting is of great significance to the energy conservation and emission reduction of automobiles. In addition, for safety reasons, the automotive industry uses a large number of high-strength steel plates. Cold-rolled high-strength steel mainly includes DP steel, DH steel, TRIP steel, CP steel and MS steel, which are mainly achieved by adding alloy elements, increasing the rapid cooling rate, and using phase transformation strengthening. Cold-rolled martensitic steel is the highest commercial cold-rolled advanced high-strength steel grade. From the lowest 900MPa to the highest strength of 1700MPa, it has ultra-high strength and excellent bending properties. It is usually used in automobile anti-collision beams, bumpers and other safety components. In recent years, the proportion of high-strength steel used in automobiles has increased year by year. The application of thin-gauge high-strength martensitic steel products has provided the automotive industry with broad space for lightweighting, reducing energy consumption and improving fuel economy.

[0003] Cold-rolled martensitic steel is usually made into corresponding parts by roller pressing. The cross-section is relatively simple, but the bending performance requirements are high. Therefore, whether it has good bending performance is the key to whether martensitic steel can be promoted and applied in large quantities. Summary of the invention

[0004] The present application provides a 1300MPa grade cold-rolled martensitic steel with high bending performance and a preparation method thereof, in order to solve the following technical problem: how to improve the bending performance of 1300MPa grade cold-rolled martensitic steel.

[0005] In a first aspect, the present application provides a method for preparing a 1300 MPa grade cold-rolled martensitic steel with high bending performance, the method comprising:

[0006] A cold hardened plate with a set chemical composition is obtained;

[0007] The chilled plate is continuously annealed to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance;

[0008] The method of continuously annealing the chilled plate to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance comprises:

[0009] The chilled plate is first heated to a first temperature, and a surface layer of the chilled plate having the first temperature is pre-oxidized under a first dew point condition, and a first heat preservation is performed under the first temperature condition to obtain a first annealed plate;

[0010] The first annealing sheet is heated to a second temperature for a second time, and is kept warm for a second time under the condition of the second temperature, and then slowly cooled and rapidly cooled to obtain a second annealing sheet;

[0011] The second annealed sheet is thirdly heated to a third temperature and aged under the condition of a first set time to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance.

[0012] Optionally, the first temperature is 640°C to 680°C, the first insulation time is 30s to 180s, and the first dew point is (-30)°C to (-20)°C.

[0013] Optionally, the second temperature is (Ac3+10)°C to (Ac3+30)°C, and the second insulation time is 180s to 360s.

[0014] Optionally, the third temperature is 200°C to 280°C, and the first set time is 300s to 600s.

[0015] Optionally, the slow cooling process parameters include: a cooling rate of 1°C / s to 15°C / s, an end point temperature of 700°C to 800°C; and / or,

[0016] The process parameters of the rapid cooling include: the cooling medium is a gas containing 50% volume fraction of hydrogen, the cooling rate is

[0017] ≥45℃ / s, the end temperature is (Ms-20)℃~(Ms-10)℃.

[0018] Optionally, the heating rate of the first heating is 2°C / s to 5°C / s; and / or,

[0019] The heating rate of the second heating is 3°C / s to 8°C / s; and / or,

[0020] The heating rate of the third heating is ≥2°C / s.

[0021] Optionally, the setting of chemical composition includes:

[0022] C, Si, Mn, P, S, Cr, B, N and Fe; among them, in terms of mass fraction,

[0023] The content of C is 0.12% to 0.18%, the content of Si is 0.2% to 0.8%, the content of Mn is 1.5% to 2.5%, the content of P is ≤0.015%, the content of S is ≤0.008%, the content of Cr is 0.3% to 0.6%, the content of B is 0.001% to 0.002%, and the content of N is 0.003% to 0.005%;

[0024] And also includes at least one of the following chemical components: Nb, Ti, V; wherein,

[0025] The content of Nb is 0.01% to 0.04%, the content of Ti is 0.01% to 0.04%, and the content of V is 0.01% to 0.04%.

[0026] Optionally, the step of obtaining a cold hardened plate having a set chemical composition comprises:

[0027] Continuously casting the molten steel to obtain a slab;

[0028] Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil;

[0029] The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein:

[0030] The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or,

[0031] The heating temperature is 1120°C to 1220°C; and / or,

[0032] The final rolling temperature of the rolling is 890°C to 920°C; and / or,

[0033] The coiling temperature is 550°C to 600°C.

[0034] In a second aspect, the present application provides a 1300 MPa grade cold-rolled martensitic steel with high bending performance prepared by the method described in the first aspect.

[0035] Optionally, the cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1300MPa, yield strength 1030MPa-1300MPa, elongation A80≥3%, and bending performance meets the requirement of bending 180°2t parallel to the rolling direction without cracking;

[0036] The microstructure of the cold-rolled martensitic steel includes lath martensite and ferrite; wherein,

[0037] The volume fraction of the lath martensite is 92% to 96%, and the volume fraction of the ferrite is 4% to 8%.

[0038] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0039] The preparation method of the 1300MPa grade cold-rolled martensitic steel with high bending performance provided in an embodiment of the present application includes: obtaining a chilled plate with a set chemical composition; continuously annealing the chilled plate, including: first heating the chilled plate to a first temperature, and pre-oxidizing the surface of the chilled plate with the first temperature under the condition of a first dew point, and performing a first heat preservation under the condition of the first temperature to obtain a first annealed plate; second heating the first annealed plate to a second temperature, and performing a second heat preservation under the condition of the second temperature, and then performing slow cooling and rapid cooling to obtain a second annealed plate; third heating the second annealed plate to a third temperature, and performing overaging under the condition of a first set time to obtain a 1300MPa grade cold-rolled martensitic steel with high bending performance. The chilled plate with set chemical composition is first heated to the first temperature and first heat-insulated, so that the chilled plate can be fully tempered, so that the structure of the chilled plate is uniform, so that the ferrite grains in different parts of the chilled plate will undergo more sufficient recrystallization, the grain difference of ferrite will be smaller, and at the same time, the martensite will undergo more sufficient tempering and transform into equiaxed ferrite and granular cementite, and the pearlite will also undergo more obvious spheroidization. Since the grain boundary is a fast diffusion channel for carbon atoms, carbon atoms will gradually diffuse to the original carbon-poor ferrite area during the first heat-insulating process, so as to achieve uniform distribution of carbide particles; the first temperature matches the first dew point, and a decarburized layer can be formed on the shallow surface of the steel plate, and a layer of ferrite structure will be formed on the inner and outer surfaces, which can withstand large changes. shape, thereby improving the bending properties of martensitic steel; second heating to the second temperature and second insulation, the organization of the cold hardened plate is completely austenitized, the fibrous microstructure completes the recovery and recrystallization process, and is completely transformed into austenite, while the residual cementite is fully dissolved, the components and microstructures in the austenite are fully homogenized, and the carbides are fully precipitated, thereby improving the bending properties; slow cooling can inhibit the formation of new ferrite; fast cooling can promote the transformation of austenite to martensite, obtain an appropriate amount of martensitic organizational structure, and thus ensure a tensile strength of more than 1300MPa; third heating to the third temperature, and over-aging under the conditions of the first set time, can promote the tempering of martensite, further improve the plastic toughness of martensite, thereby improving the bending properties. In summary, the bending properties of 1300MPa grade cold-rolled martensitic steel are improved through the synergistic effect of chemical composition design and control of continuous annealing process parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0041] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0042] Figure 1 A schematic flow chart of a method for preparing a 1300 MPa grade cold-rolled martensitic steel with high bending performance according to some embodiments of the present application;

[0043] Figure 2 A microstructure diagram of a 1300MPa grade cold-rolled martensitic steel with high bending performance provided according to some embodiments of the present application;

[0044] Figure 3 This is a picture of the bending test results of a 1300MPa grade cold-rolled martensitic steel with high bending performance provided according to some embodiments of the present application. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0046] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0047] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0048] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0049] Figure 1 A schematic diagram of a process for preparing a 1300 MPa grade cold-rolled martensitic steel with high bending performance according to some embodiments of the present application; see Figure 1 The present application provides a method for preparing a 1300MPa grade cold-rolled martensitic steel with high bending performance, the method comprising:

[0050] S1, obtaining a cold hardened plate with a set chemical composition;

[0051] In some embodiments, the setting of the chemical composition comprises:

[0052] C, Si, Mn, P, S, Cr, B, N and Fe; among them, in terms of mass fraction,

[0053] The content of C is 0.12% to 0.18%, the content of Si is 0.2% to 0.8%, the content of Mn is 1.5% to 2.5%, the content of P is ≤0.015%, the content of S is ≤0.008%, the content of Cr is 0.3% to 0.6%, the content of B is 0.001% to 0.002%, and the content of N is 0.003% to 0.005%;

[0054] And also includes at least one of the following chemical components: Nb, Ti, V; wherein,

[0055] The content of Nb is 0.01% to 0.04%, the content of Ti is 0.01% to 0.04%, and the content of V is 0.01% to 0.04%.

[0056] In the embodiment of the present application, the C element is the most important solid solution strengthening element and the element for improving the hardenability of austenite in martensitic steel. In order to obtain sufficient martensite in the cooling process to ensure a tensile strength of more than 1300 MPa, C forms carbonitrides with microalloying Nb and Ti elements during the heat treatment process, refines the grains, helps to obtain a yield strength of more than 1030 MPa, and avoids excessive C content from deteriorating welding performance. Exemplarily, the above C content can be 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, etc.

[0057] Si is also an important solid solution strengthening element. At the same time, Si can effectively promote the enrichment of C elements into austenite, improve the hardenability of austenite, purify the ferrite phase, and improve the elongation. Si also helps to inhibit the formation of carbides during the tempering process after cooling, thereby improving the bending performance of the steel plate. However, Si is an important element that causes iron oxide scale to form on the surface of hot-rolled plates. Too high Si content will cause residual iron oxide scale after pickling, which will deteriorate the surface quality of the continuous annealing plate. Exemplarily, the above-mentioned Si content can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, etc.

[0058] Mn is an austenite stabilizing element. During the annealing process, it can diffuse from ferrite to austenite, improve the stability of austenite and improve hardenability. In addition, Mn can improve the strength of martensite through solid solution strengthening, ensuring a high yield strength of more than 1030MPa and a high tensile strength of more than 1300MPa. However, Mn increases the deterioration of bending properties, and the formation of MnS inclusions often becomes the starting point for cracks during bending, so the manganese content should not be too high. And too high a Mn content can easily cause structural segregation, which can easily lead to bending cracking and deteriorate the comprehensive properties of steel. At the same time, it will also enrich the surface during the annealing process, so the Mn content should not be too high. Exemplarily, the above-mentioned Mn content can be 1.5%, 1.7%, 1.9%, 2.1%, 2.3%, 2.5%, etc.

[0059] The Cr element can improve the hardenability of austenite, thereby obtaining a sufficient amount of martensite, obtaining a tensile strength of more than 1300 MPa, and ensuring that the alloy manufacturing cost is sufficiently low; but at the same time, the Cr element is a ferrite zone expansion element, and too much Cr element will cause the two-phase zone to shrink and hinder the bainite transformation. Exemplarily, the Cr content can be 0.3%, 0.4%, 0.5%, 0.6%, etc.

[0060] As an interstitial solid solution atom, P can appropriately improve the strength of the steel plate, but it is also easy to segregate at the grain boundary and deteriorate the plasticity and formability. For example, the content of P can be 0.015%, 0.013%, 0.010%, etc.

[0061] S is easy to combine with Mn to form coarse MnS inclusions, which deteriorate the bending performance of the steel plate. For example, the S content can be 0.008%, 0.007%, 0.006%, etc.

[0062] B plays a very important role in improving the hardenability of the steel plate during the cooling process. When the B content is too low, it is difficult to achieve grain boundary strengthening, and grain boundary strengthening is required to obtain excellent delayed fracture resistance. In addition, since B diffuses to the grain boundary significantly faster than P, it prevents the adverse effects of P segregation on the grain boundary, and P segregation will deteriorate the bendability of the steel. However, when the B content is too high, carboride is easily formed, which is not conducive to performance improvement. Exemplarily, the above-mentioned B content can be 0.001%, 0.0013%, 0.0015%, 0.0018%, 0.002%, etc.

[0063] N can reduce the nitride precipitates in the steel, thereby reducing the formation of irreversible hydrogen trap second phase particles. In addition, it also makes the original austenite grain boundaries coarser, reduces the number of grain boundaries, increases the tendency of crack propagation, and ultimately leads to deterioration of bending performance. However, when the N content is too high, the nitrides in the steel coarsen, thereby reducing the grain pinning effect and causing deterioration of the bending performance of the steel. Exemplarily, the above-mentioned N content can be 0.003%, 0.0035%, 0.004%, 0.0045%, 0.005%, etc.

[0064] The Nb element not only has a significant grain refinement effect, but is also a strong carbide-forming element, which can improve the yield strength of martensitic steel through precipitation strengthening. However, Nb significantly inhibits recrystallization. Too high a Nb content will cause the annealing stage to enter the non-recrystallization zone, resulting in the formation of a deformation band along the rolling direction of the organization, causing the bending performance to deteriorate. Like Nb, Ti is also a strong carbide-forming element, which can improve the yield strength through precipitation strengthening. At the same time, Ti is beneficial for refining grains and obtaining a uniform equiaxed microstructure. In addition, the cost of Ti is lower than that of Nb. However, excessive addition of Ti leads to increased costs. V has a similar effect to Nb and Ti, forming carbides or carbonitrides to promote organizational refinement and enhance the strength of steel. Exemplarily, the chemical composition may contain one or more of Nb, Ti, and V; the contents of Nb, Ti, and V may all be 0.01%, 0.02%, 0.03%, 0.04%, etc.

[0065] In some embodiments, obtaining a cold hardened plate having a set chemical composition comprises:

[0066] Continuously casting the molten steel to obtain a slab;

[0067] Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil;

[0068] The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein:

[0069] The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or,

[0070] The heating temperature is 1120°C to 1220°C; and / or,

[0071] The final rolling temperature of the rolling is 890°C to 920°C; and / or,

[0072] The coiling temperature is 550°C to 600°C.

[0073] In an embodiment of the present application, the above-mentioned rolling specifically includes: rough descaling, rough rolling, induction heating, fine descaling, finishing rolling, and laminar cooling; the hot-rolled coil can be air-cooled and then cold-rolled; the above-mentioned finishing rolling adopts any one of single-bill rolling, semi-headless rolling and headless rolling, and prepares high bending performance 1300MPa grade cold-rolled martensitic steel based on a multi-mode thin slab continuous casting and rolling production line.

[0074] The casting speed and thickness of the continuous casting are limited to ensure the production rhythm and avoid leakage during endless rolling. For example, the casting speed of the continuous casting can be 4m / min, 5m / min, 6m / min, 7m / min, etc.; the thickness of the slab can be 110mm, 115mm, 120mm, 125mm, etc.

[0075] By limiting the heating temperature, the alloy elements of the slab can be homogenized. By limiting the final rolling temperature of rolling and the temperature of coiling, the structure of the heated slab can be homogenized. Exemplarily, the heating temperature can be 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, etc.; the final rolling temperature of the rolling can be 890°C, 900°C, 910°C, 920°C, etc., and the coiling temperature can be 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, etc.

[0076] S2, continuously annealing the chilled plate to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance;

[0077] The method of continuously annealing the chilled plate to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance comprises:

[0078] The chilled plate is first heated to a first temperature, and a surface layer of the chilled plate having the first temperature is pre-oxidized under a first dew point condition, and a first heat preservation is performed under the first temperature condition to obtain a first annealed plate;

[0079] The first annealing sheet is heated to a second temperature for a second time, and is kept warm for a second time under the condition of the second temperature, and then slowly cooled and rapidly cooled to obtain a second annealing sheet;

[0080] The second annealed sheet is thirdly heated to a third temperature and aged under the condition of a first set time to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance.

[0081] In some embodiments, the first temperature is 640°C to 680°C, the first insulation time is 30s to 180s, and the first dew point is (-30)°C to (-20)°C.

[0082] In some embodiments, the heating rate of the first heating is 2°C / s to 5°C / s; and / or,

[0083] The heating rate of the second heating is 3°C / s to 8°C / s; and / or,

[0084] The heating rate of the third heating is ≥2°C / s.

[0085] In the embodiment of the present application, based on the above-mentioned set chemical composition, the process parameters in the continuous annealing are controlled to achieve the optimization of the target structure. The heating rate of the first heating is limited to balance the residence time of the cold hard plate in the continuous annealing furnace, so that the C / Mn elements can be fully diffused, the recovery recrystallization is sufficient, and the structure is homogenized. Exemplarily, the heating rate of the first heating can be 2℃ / s, 3℃ / s, 4℃ / s, 5℃ / s, etc.

[0086] The first heat preservation is carried out under the condition of the first temperature (below Ac1), and the cold-rolled sheet is further subjected to sufficient high-temperature tempering to achieve the purpose of structural homogenization, so that the ferrite grains in different parts will undergo more sufficient recrystallization, and the grain difference of ferrite will become smaller; at the same time, the martensite will undergo more sufficient tempering and transform into equiaxed ferrite and granular cementite; pearlite will also undergo more obvious spheroidization. Since the grain boundary is a fast diffusion channel for carbon atoms, carbon atoms will gradually diffuse to the original carbon-poor ferrite area during the first heat preservation to achieve a uniform distribution of carbide particles. The above-mentioned pre-oxidation has the effect of inhibiting the external oxidation of elements such as Si to achieve good phosphating performance, and it is also beneficial to form a decarburized layer on the shallow surface of the steel plate, which is beneficial to the improvement of bending performance. During the cold bending process, the deformation of the inner and outer surfaces of the bending sample is the largest, the outer surface is stretched, and the inner surface is compressed. If the surface is decarburized, a layer of ferrite structure will be formed on both the inner and outer surfaces. Compared with the hard phase martensite structure, the soft phase ferrite has better plasticity and can bear larger deformation, thereby improving the bending performance of the martensitic steel. If the first dew point is too low, the oxygen partial pressure is likely to be insufficient, which is not conducive to obtaining a decarburized layer; if the first dew point is too high, the decarburization is too serious, the surface hardness of the steel plate decreases, and the formability of the steel plate is not conducive. Exemplarily, the first temperature can be 640°C, 650°C, 660°C, 670°C, 680°C, etc., the first insulation time can be 30s, 50s, 70s, 100s, 120s, 150s, 170s, 180s, etc., and the first dew point can be -20°C, -22°C, -24°C, -25°C, -26°C, -28°C, -30°C, etc.

[0087] In some embodiments, the second temperature is (Ac3+10)°C to (Ac3+30)°C, and the second insulation time is 180s to 360s.

[0088] The heating rate of the second heating is limited. When heating at a higher temperature, the heating rate needs to be further increased to heat the steel plate to the second temperature in a short time. After heating to above the Ac1 point, the reverse transformed austenite will be evenly distributed in the matrix, thereby eliminating the hereditary unevenness of the original organization, which is beneficial to improving the bending performance of the finished product. Exemplarily, the heating rate of the second heating can be 6°C / s, 3°C / s, 4°C / s, 5°C / s, 7°C / s, 8°C / s, etc.

[0089] The second insulation (heating stage) is carried out under the second temperature condition, which can make the structure completely austenitized, and the fibrous microstructure completes the recovery and recrystallization process and is completely transformed into austenite. At the same time, the residual cementite is fully dissolved, the components and microstructure in the austenite are fully homogenized, and the carbides of Nb and Ti are fully precipitated, which effectively improves the bending performance of the finished product while ensuring a tensile strength of more than 1300MPa. Exemplarily, the second temperature can be (Ac3+10)°C, (Ac3+12)°C, (Ac3+14)°C, (Ac3+16)°C, (Ac3+180°C, (Ac3+20)°C, (Ac3+25)°C, (Ac3+23)°C, (Ac3+28)°C, (Ac3+30)°C, etc., and the second insulation time can be 180s, 200s, 220s, 240s, 260s, 280s, 300s, 320s, 340s, 360s, etc.

[0090] In some embodiments, the third temperature is 200° C. to 280° C., and the first set time is 300 s to 600 s.

[0091] In the embodiment of the present application, during cold bending deformation, cracks in the steel plate are most likely to occur at the interface between two phases with a large difference in hardness. The cold bending performance is closely related to the uniformity of the organization, and the uniformity of the organization of cold-rolled martensitic steel mainly includes the distribution and hardness of inclusions and martensite phases in the steel plate. Low-temperature overaging in the overaging stage basically does not affect the morphology and distribution of martensite, but only affects its hardness. It can be seen that appropriately increasing the overaging temperature can reduce the hardness of martensite and the hardness difference between martensite and ferrite, which is beneficial to the improvement of the cold bending performance of martensitic steel. If the overaging temperature is too low or the overaging time is too short, it is not conducive to the tempering of martensite, the plasticity of martensite is poor, and the bending performance is deteriorated; if the overaging temperature is too high or the overaging time is too long, it will promote the precipitation of cementite and deteriorate the bending formability. Limiting the third heating temperature rise rate is beneficial to improving the plasticity of martensite. Exemplarily, the third temperature may be 200°C, 220°C, 240°C, 260°C, 270°C, 280°C, etc., and the first setting time may be 300s, 350s, 400s, 450s, 500s, 550s, 600s, etc.; the third heating temperature rise rate may be 2°C / s, 2.5°C / s, 3°C / s, etc.

[0092] In some embodiments, the slow cooling process parameters include: a cooling rate of 1°C / s to 15°C / s, an end point temperature of 700°C to 800°C; and / or,

[0093] The process parameters of the rapid cooling include: the cooling medium is a gas containing 50% volume fraction of hydrogen, the cooling rate is

[0094] ≥45℃ / s, the end temperature is (Ms-20)℃~(Ms-10)℃.

[0095] In the embodiment of the present application, the process parameters of slow cooling are limited to ensure that the formation of new ferrite can be suppressed during the initial cooling process, which can not only avoid the evolution of microstructure inhomogeneity, but also avoid the reduction of austenite hardenability caused by the enrichment of carbon in austenite. The process parameters of rapid cooling are limited, and the terminal temperature of rapid cooling is below the martensitic phase transformation temperature. Combined with the cooling medium and cooling rate of rapid cooling, the transformation of austenite to martensite is promoted to obtain a 92-96% martensitic structure and a 4-8% ferrite structure. Exemplarily, in the above-mentioned slow cooling process parameters, the cooling rate can be 1°C / s, 3°C / s, 5°C / s, 7°C / s, 9°C / s, 11°C / s, 13°C / s, 15°C / s, etc.; the terminal temperature can be 700°C, 720°C, 740°C, 760°C, 780°C, 800°C, etc. Among the above-mentioned rapid cooling process parameters, the cooling rate can be 45°C / s, 46°C / s, 47°C / s, 48°C / s, 49°C / s, etc.; the terminal temperature can be (Ms-20)°C, (Ms-10)°C, (Ms-15)°C, (Ms-13)°C, (Ms-18)°C, etc.

[0096] In a second aspect, the present application provides a 1300 MPa grade cold-rolled martensitic steel with high bending performance prepared by the method described in the first aspect.

[0097] In some embodiments, the cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1300MPa, yield strength 1030MPa-1300MPa, elongation A80≥3%, and bending performance meets the requirement of bending 180°2t parallel to the rolling direction without cracking;

[0098] The microstructure of the cold-rolled martensitic steel includes lath martensite and ferrite. Figure 2 For a microstructure diagram of a 1300MPa grade cold-rolled martensitic steel with high bending performance provided according to some embodiments of the present application, please refer to Figure 2 ;in,

[0099] The volume fraction of the lath martensite is 92% to 96%, and the volume fraction of the ferrite is 4% to 8%.

[0100] In an embodiment of the present application, the 1300MPa grade cold-rolled martensitic steel has excellent strength properties and bending properties. The volume fraction of the lath martensite can be 92%, 93%, 94%, 95%, 96%, etc., and the volume fraction of the ferrite can be 4%, 5%, 6%, 7%, 8%, etc.

[0101] The 1300MPa grade cold-rolled martensitic steel with high bending performance is realized based on the above-mentioned preparation method of the 1300MPa grade cold-rolled martensitic steel with high bending performance. The specific steps of the preparation method of the 1300MPa grade cold-rolled martensitic steel with high bending performance can refer to the above-mentioned embodiment. Since the 1300MPa grade cold-rolled martensitic steel with high bending performance adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0102] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0103] The embodiment of the present application provides a 1300 MPa grade cold-rolled martensitic steel with high bending performance. Please refer to the chemical composition of the 1300 MPa grade cold-rolled martensitic steel with high bending performance shown in Table 1, the preparation process parameters of the cold-hardened plate shown in Table 2, the continuous annealing process parameters of the cold-hardened plate shown in Table 3, and the performance results of the 1300 MPa grade cold-rolled martensitic steel with high bending performance shown in Table 4.

[0104] Table 1 Chemical composition of 1300MPa grade cold-rolled martensitic steel with high bending performance (wt%)

[0105]

[0106] Table 2 Preparation process parameters of cold hardened plate

[0107]

[0108] Table 3 Process parameters of continuous annealing of cold hardened plate

[0109]

[0110]

[0111] The performance of the 1300 MPa grade cold-rolled martensitic steel with high bending performance prepared in Examples 1 to 6 and Comparative Examples 1 to 4 was tested, see Table 4.

[0112] The tensile strength Rm, yield strength Rp0.2 and A80 in Table 4 are evaluated using GBT 228.1-2021 Tensile tests on metallic materials Part 1: Room temperature test method.

[0113] The bending test is carried out using the GBT 232-2010 metal material bending test method, where R is the bending core radius, t is the thickness of the steel plate, and the steel is qualified if there is no visible crack on the outer side after bending.

[0114] Table 4 Performance results of high bending performance 1300MPa grade cold rolled martensitic steel.

[0115]

[0116]

[0117] In summary, the high bending performance 1300MPa grade cold-rolled martensitic steel prepared by the embodiment of the present application meets the following mechanical properties: tensile strength>1300MPa, yield strength 1030MPa~1300MPa, elongation A80≥3%, and the bending performance satisfies the requirement of bending 180°2t parallel to the rolling direction without cracking, and at the same time has excellent strength and bending properties. Figure 3 For a picture of the bending test results of a 1300MPa grade cold-rolled martensitic steel with high bending performance provided according to some embodiments of the present application, please refer to Figure 3 , indicating that the 1300MPa grade cold-rolled martensitic steel provided in the embodiment of the present application has excellent bending properties. However, the second temperature of Comparative Example 1 is too low; Comparative Example 2 is directly heated to the second temperature; Comparative Example 3 is over-aged at the final cooling temperature of rapid cooling, and the over-aging temperature is low; Comparative Example 4 has too low C content, which makes the performance of the cold-rolled martensitic steel inferior to that of the embodiment to a certain extent.

[0118] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing 1300MPa grade cold-rolled martensitic steel with high bending performance, It is characterized in that The method comprises: A cold hardened plate with a set chemical composition is obtained; The chilled plate is continuously annealed to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance; The method of continuously annealing the chilled plate to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance comprises: The chilled plate is first heated to a first temperature, and a surface layer of the chilled plate having the first temperature is pre-oxidized under a first dew point condition, and a first heat preservation is performed under the first temperature condition to obtain a first annealed plate; The first annealing sheet is heated to a second temperature for a second time, and is kept warm for a second time under the condition of the second temperature, and then slowly cooled and rapidly cooled to obtain a second annealing sheet; The second annealed sheet is thirdly heated to a third temperature and aged under the condition of a first set time to obtain a 1300 MPa grade cold-rolled martensitic steel with high bending performance.

2. The method according to claim 1, It is characterized in that The first temperature is 640°C to 680°C, the first insulation time is 30s to 180s, and the first dew point is (-30)°C to (-20)°C.

3. The method according to claim 1, It is characterized in that The second temperature is (Ac3+10)°C to (Ac3+30)°C, and the second insulation time is 180s to 360s.

4. The method according to claim 1, It is characterized in that The third temperature is 200° C. to 280° C., and the first set time is 300s to 600s.

5. The method according to claim 1, It is characterized in that The process parameters of the slow cooling include: a cooling rate of 1°C / s to 15°C / s, an end point temperature of 700°C to 800°C; and / or, The process parameters of the rapid cooling include: the cooling medium is a gas containing 50% volume fraction of hydrogen, the cooling rate is ≥45°C / s, and the end point temperature is (Ms-20)°C to (Ms-10)°C.

6. The method according to claim 1, It is characterized in that The heating rate of the first heating is 2°C / s to 5°C / s; and / or, The heating rate of the second heating is 3°C / s to 8°C / s; and / or, The heating rate of the third heating is ≥2°C / s.

7. The method according to any one of claims 1 to 6, It is characterized in that The set chemical composition includes: C, Si, Mn, P, S, Cr, B, N and Fe; among them, in terms of mass fraction, The content of C is 0.12% to 0.18%, the content of Si is 0.2% to 0.8%, the content of Mn is 1.5% to 2.5%, the content of P is ≤0.015%, the content of S is ≤0.008%, the content of Cr is 0.3% to 0.6%, the content of B is 0.001% to 0.002%, and the content of N is 0.003% to 0.005%; And also includes at least one of the following chemical components: Nb, Ti, V; wherein, The content of Nb is 0.01% to 0.04%, the content of Ti is 0.01% to 0.04%, and the content of V is 0.01% to 0.04%.

8. The method according to claim 1, It is characterized in that The method of obtaining a cold hardened plate with a set chemical composition comprises: Continuously casting the molten steel to obtain a slab; Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil; The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein: The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or, The heating temperature is 1120° C. to 1220° C.; and / or, The final rolling temperature of the rolling is 890°C to 920°C; and / or, The coiling temperature is 550°C to 600°C.

9. A 1300 MPa grade cold-rolled martensitic steel with high bending performance prepared by the method according to any one of claims 1 to 8.

10. The cold rolled martensitic steel according to claim 9, It is characterized in that The cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1300MPa, yield strength 1030MPa-1300MPa, elongation A80≥3%, and bending performance meets the requirement of bending 180°2t parallel to the rolling direction without cracking; The microstructure of the cold-rolled martensitic steel includes lath martensite and ferrite; wherein, The volume fraction of the lath martensite is 92% to 96%, and the volume fraction of the ferrite is 4% to 8%.

Citation Information

Patent Citations

  • High-bending 980MPa cold rolled dual-phase steel and its preparation technology

    CN102828119A

  • 1200MPa-grade ultra-fast cold-rolled double-phase steel plate and preparation method thereof

    CN109280857A

  • Ultra-high strength steel sheet having excellent bendability and manufacturing method therefor

    CN110073024A

  • Ultrahigh-strength martensitic steel as well as preparation method and application thereof

    CN111519109A

  • Low-cost 1200Mpa-grade cold-rolled high-strength martensitic steel and manufacturing method thereof

    CN114086071A