Method for recovering iron and aluminum from high-iron bauxite through direct reduction, electric furnace smelting and magnetic separation
Through the direct reduction of high-speed rail bauxite, electric furnace smelting-magnetic separation and recovery of iron and aluminum, the waste of resources and environmental pollution caused by the close glued structure of iron and aluminum in high-speed rail bauxite is solved, and high-purity alumina and ferrosilicon alloys are realized. Efficient separation and recycling, simplifying process flow and improving yield and purity.
Patent Information
- Application Number
- CN202411049054.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing comprehensive utilization process of high-speed rail bauxite has problems such as polluting the environment, low product purity and low product output, especially the high-speed rail bauxite content has not been effectively utilized, resulting in waste of resources and environmental pollution.
The method of direct reduction of high-speed rail bauxite-electric furnace smelting-magnetic separation and recovery of iron and aluminum is adopted. By crushing and fine grinding, it is mixed with reduced coal, and gas phase direct reduction and magnetic separation are carried out, and the arc furnace smelting and magnetic separation equipment are separated out. High-purity alumina and ferrosilicon alloys destroy the close glued structure of iron and aluminum and improve the separation efficiency of aluminum and iron.
It realizes efficient separation of high-purity alumina and high-quality ferrosilicon alloys, improves product purity and output, simplifies process flow, reduces equipment investment and energy consumption, and is suitable for industrial production.
Smart Images

Figure CN118979147A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ore smelting, and in particular to a method for recovering iron and aluminum through direct reduction of high-iron bauxite, electric furnace smelting and magnetic separation. Background Art
[0002] With the exploitation and utilization of resources, the high-quality bauxite resources are now scarce, but the low-quality low-aluminum high-iron bauxite resources are currently abundant. The rational development and utilization of low-aluminum high-iron bauxite is currently a way to solve the shortage of high-quality bauxite resources. The microcrystalline structure of iron and aluminum closely bonded in high-iron bauxite is one of the main technical difficulties restricting its efficient utilization. In the development and application of bauxite, bauxite with high iron content often leads to the failure to effectively utilize its reserves and brings environmental and other problems.
[0003] At present, the comprehensive utilization process of high-iron bauxite mainly includes two methods: wet method and dry method. The wet process mainly includes two methods: acid method and alkaline method. The acid method is a traditional method for comprehensive utilization of bauxite. Its main process is to first dissolve aluminum, sodium and other metal ions in bauxite with leaching acid, and then separate and purify them with carbonate precipitation method. The acid process has the advantages of simple operation, mature process, and high product purity, but it also has the disadvantages of leaching wastewater treatment problems and high energy consumption; the core of the alkaline process is to dissolve aluminum ions in bauxite with sodium hydroxide, and then neutralize them with acidic solutions such as hydrochloric acid, and finally separate and purify them with carbonate method. The advantages of the alkaline process are energy saving and environmental protection, and small wastewater discharge, but it also has the disadvantages of low product purity and low product output. The dry process is mainly based on the thermal decomposition of bauxite, which decomposes bauxite at high temperature to produce products such as aluminate and iron oxide. The advantages of the dry process are energy saving and environmental protection, no wastewater discharge, and no need for large amounts of chemical agents. However, it also has disadvantages such as complex process, large equipment investment, and low product purity.
[0004] In view of the above problems, the present invention proposes a method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation. Summary of the invention
[0005] The purpose of the present invention is to provide a method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation, so as to solve the problems of environmental pollution, low product purity and low product yield raised in the above background technology.
[0006] To achieve the above object, the present invention provides a method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation, which specifically comprises the following steps:
[0007] S1. crushing and grinding high iron bauxite and reduced coal ore and mixing them evenly;
[0008] S2, placing the mixture of high-iron bauxite and reduced coal into a tubular furnace filled with nitrogen for reduction;
[0009] S3, performing weak magnetic separation on the reduced ore to screen out aluminum concentrate and iron concentrate, and spreading carbon powder on and around the surface of the iron concentrate;
[0010] S4, conduct strong magnetic separation on aluminum concentrate to screen out high-quality bauxite and iron-aluminum spinel;
[0011] S5, evenly mix the high-quality bauxite and the iron ore concentrate covered with reduced coal powder and put them into an electric arc furnace for smelting, and take them out after cooling after smelting;
[0012] S6. The solidified lumps are broken up and magnetically separated by a magnetic separation device. After the magnetic separation, magnetic materials such as ferrosilicon alloy and high-purity alumina are obtained.
[0013] Preferably, in S1, the portion of the high-iron bauxite crushed to a particle size of <1 cm and finely ground to a particle size of <0.1 mm accounts for more than 50% of the total weight of the high-iron bauxite; the portion of the reduced coal finely ground to a particle size of <0.05 mm accounts for more than 70% of the total weight of the reduced coal.
[0014] Preferably, in S1, the mass ratio of high-iron bauxite to reduced coal is 100:2-10.
[0015] Preferably, in S1, the high-iron bauxite is a Ghanaian gibbsite-type high-iron bauxite, which comprises Al 2 O 3 45~55%, SiO 2 5~10%,Fe 2 O 3 30% and other unavoidable impurities.
[0016] Preferably, in S1, the reducing coal is lignite or anthracite.
[0017] Preferably, in S2, direct reduction is carried out at 1100-1400°C for 60-180 min; the reduction is carried out until the ratio of the fixed carbon content in the reduced coal to the oxygen content of the iron oxide in the iron-containing mineral is 1-3, and the nitrogen flow rate is 1.5 L / min.
[0018] Preferably, in S3, the magnetic field strength of weak magnetic separation is 90-160 mT, and the amount of carbon powder used is 5-10% of the amount of high-iron bauxite used in S1.
[0019] Preferably, in S4, the magnetic field strength is 1000-1600 mT.
[0020] Preferably, in S5, the smelting temperature is 2000-3000° C., and the smelting time is 180-360 min.
[0021] Preferably, in S6, the magnetic field strength is 100-200 mT.
[0022] In the ore grinding step, the present invention uses high-energy mechanical equipment to grind the high-iron bauxite, break the iron-aluminum structure in the high-iron bauxite, promote the separation of aluminum and iron, and quickly reconstruct its physical phase. In the reduction process, a coal powder reducing agent is used to reduce the iron ions in the high-iron bauxite into iron particles, thereby destroying the closely bonded structure of iron and aluminum in the high-iron bauxite and promoting the separation of iron and aluminum. In terms of the use of reducing materials, materials containing reducing properties such as coke, carbon black, and charcoal are usually used. At the same time, by adjusting the intensity of the magnetic field, metallic iron, aluminum concentrate, and iron-aluminum spinel are separated in turn, and the grade of the bauxite is improved so that it meets the requirements for entering the electric arc furnace to smelt alumina. During the arc furnace smelting process, SiO 2 The coking coal reduces the Si element to Si, which reacts with the iron element to form ferrosilicon and sinks to the bottom of the molten material. 2 O 3 At the top of the molten material, magnetic separation can effectively separate iron and aluminum after crushing, leaving high-purity alumina.
[0023] Therefore, the present invention proposes a method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation. Compared with the existing high-iron bauxite comprehensive utilization method, the specific beneficial effects are as follows:
[0024] (1) Compared with separation processes such as magnetic separation, flotation, and suspended roasting, it can more effectively separate alumina and iron minerals in high-iron bauxite ore, and the separated alumina has high purity and high-quality ferrosilicon alloy.
[0025] (2) The high-iron bauxite is reduced by direct reduction-dependent gas, which has higher heat transfer efficiency than conventional roasting methods.
[0026] (3) The process flow of the present invention is simple, the equipment processing capacity is large, the product properties are easy to control, and it is easy to industrialize and realize large-scale production.
[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic flow chart of a method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to the present invention. DETAILED DESCRIPTION
[0029] The present invention provides a method for recovering iron and aluminum by direct reduction of high-iron bauxite, electric furnace smelting and magnetic separation. Figure 1 As shown, the specific steps include:
[0030] S1. Crush the high-iron bauxite to a particle size of less than 1 cm, and then grind it to a particle size of less than 0.1 mm, which accounts for more than 50% of the total weight; grind the reduced coal to a particle size of less than 0.05 mm, which accounts for more than 70% of the total weight; mix the high-iron bauxite powder and the reduced coal powder in a mass ratio of 100:2 to 10 to prepare a mixture, thereby ensuring that the ratio of the fixed carbon content in the reduced coal to the oxygen content of the iron oxide in the iron-containing mineral is 1 to 3.
[0031] In the present invention, the high-iron bauxite is a Ghanaian gibbsite-type high-iron bauxite, the main mineral component of which is gibbsite, and also includes gangue minerals, mainly aluminum goethite, hematite, kaolinite, rutile, quartz, etc. In terms of mass percentage, it includes Al 2 O 3 45~55%, SiO 2 5~10%,Fe 2 O 3 30% and other inevitable impurities, the reducing coal is lignite or anthracite; among which, the chemical composition of anthracite powder is: fixed carbon 80.12%, ash 9.37%, volatile matter 8.58% and other inevitable impurities.
[0032] S2. Place the mixture in a tubular furnace for direct reduction at a reduction temperature of 1100-1400° C. for a reduction time of 60-180 min. At the same time, nitrogen is introduced into the tubular furnace at a nitrogen flow rate of 1.5 L / min.
[0033] S3. The reduced ore is subjected to a weak magnetic separation using a dry magnetic separator with a magnetic field strength of 90 to 160 mT to separate the aluminum concentrate and iron concentrate, and a layer of carbon powder is spread on the surface and around the iron concentrate. The amount of carbon powder accounts for 5 to 10% of the total amount of the initial high-iron bauxite to ensure that the metallic iron will not be rapidly oxidized in the air.
[0034] S4. Carry out a strong magnetic separation on the aluminum concentrate to screen out high-quality bauxite and ferroaluminum spinel. The magnetic separator used here should be a dry magnetic separator with a magnetic field strength of 1000-1600mT.
[0035] In the present invention, the screened ferroaluminum spinel can be put into the S2 tube furnace for recycling. It should be noted that an appropriate amount of coal powder should be added to the tube furnace for each cycle to ensure that the ratio of the fixed carbon content in the reducing coal to the oxygen content of the iron oxide in the iron-containing mineral is 1 to 3.
[0036] S5. Evenly mix the high-quality bauxite and the iron ore concentrate covered with reduced coal powder and put them into an electric arc furnace for smelting at 2000-3000°C for 180-360 minutes. After the smelting is completed, the copper pot is taken out after cooling. The electric arc furnace mentioned here is an electric arc melting furnace.
[0037] After smelting in the present invention, the molten material is cooled and the ferrosilicon alloy is located in the lower part, and the alumina is located in the upper part. The material should be broken into two parts at a certain boundary in the middle and then finely ground respectively, so that the magnetic separation efficiency is improved and the iron and aluminum are separated more thoroughly.
[0038] S6. Break the solidified lumps and perform magnetic separation using a magnetic separation device. The magnetic separation device referred to here is a wet magnetic separator or a dry magnetic separator, and the magnetic field strength is 100 to 200 mT.
[0039] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, and simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0040] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0041] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0042] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.
[0043] Example 1
[0044] This embodiment provides a method for recovering iron and aluminum through direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation. The ore used in this embodiment is Ghanaian gibbsite-type high-iron bauxite, in which the useful mineral is gibbsite, and the gangue minerals are mainly aluminum goethite, hematite, kaolinite, rutile, quartz, etc., which contain Al by mass percentage. 2 O 3 51.5%, SiO 2 9.8%,Fe2 O 3 30.3% and other inevitable impurities, belonging to gibbsite-type high-iron bauxite.
[0045] The specific steps are as follows:
[0046] The high-iron bauxite ore was crushed to a particle size of less than 1 cm by a jaw crusher, and the high-speed multifunctional pulverizer was finely ground to a particle size of less than 0.1 mm, accounting for 50% of the total weight; the reduced coal was finely ground to a particle size of less than 0.1 mm, accounting for 70% of the total weight, to obtain reduced coal powder. The high-iron bauxite and coal powder were put into a ball mill at a mass ratio of 100:3.7 and ground to a particle size of ≤0.074 mm, accounting for 50%, to obtain a mixture. The mixture was placed in a tubular furnace for reduction reaction, first evacuated to vacuum, and then nitrogen was introduced at a flow rate of 1.5L / min, and moderate direct reduction was carried out at 1100°C for 180 minutes to obtain reduced ore. The reduced ore is placed in a magnetic separator for the first stage of weak magnetic separation with a magnetic field strength of 90mT to obtain iron concentrate and aluminum concentrate, and carbon powder accounting for 5% of the total mass of the initial ore powder is spread on the surface and around the iron concentrate; the aluminum concentrate is subjected to the second stage of strong magnetic separation with a magnetic field strength of 1000mT; the iron concentrate and high-quality bauxite covered with coal powder are put into an arc smelting furnace and smelted at 2200℃ for 360min; after the smelting is completed, the copper crucible is cooled with the furnace, and the molten material is broken after cooling and solidification, and magnetic separation is carried out through a magnetic separation tube with a magnetic field strength of 200mT.
[0047] The final aluminum oxide obtained has a purity of 95.7% and a high-quality ferrosilicon alloy with a Fe / Si ratio of 1.4.
[0048] Example 2
[0049] This embodiment provides a method for recovering iron and aluminum through direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation. The ore used in this embodiment is Ghanaian gibbsite-type high-iron bauxite, in which the useful mineral is gibbsite, and the gangue minerals are mainly aluminum goethite, hematite, kaolinite, rutile, quartz, etc., which contain Al by mass percentage. 2 O 3 49.5%, SiO 2 10.2%,Fe 2 O 3 29.5% and other inevitable impurities, belonging to gibbsite-type high-iron bauxite.
[0050] The specific steps are as follows:
[0051] The high-iron bauxite ore was crushed to a particle size of less than 1 cm by a jaw crusher, and the high-speed multifunctional pulverizer was finely ground to a particle size of less than 0.1 mm, accounting for 50% of the total weight; the reduced coal was finely ground to a particle size of less than 0.1 mm, accounting for 70% of the total weight, to obtain reduced coal powder. The high-iron bauxite and coal powder were put into a ball mill at a mass ratio of 100:5.2 and ground to a particle size of ≤0.074 mm, accounting for 60%, to obtain a mixture. The mixture was placed in a tubular furnace for reduction reaction, first evacuated to vacuum, and then nitrogen was introduced at a flow rate of 1.5L / min, and moderate direct reduction was carried out at 1200°C for 150 minutes to obtain reduced ore. The reduced ore is placed in a magnetic separator for the first stage of weak magnetic separation with a magnetic field strength of 120mT to obtain iron concentrate and aluminum concentrate, and carbon powder accounting for 5% of the total mass of the initial ore powder is spread on the surface and around the iron concentrate; the aluminum concentrate is subjected to the second stage of strong magnetic separation with a magnetic field strength of 1200mT; the iron concentrate and high-quality bauxite covered with coal powder are put into an arc smelting furnace and smelted at 2500℃ for 300min; after the smelting is completed, the copper crucible is cooled with the furnace, and the molten material is broken after cooling and solidification, and magnetic separation is carried out through a magnetic separation tube with a magnetic field strength of 180mT.
[0052] The final aluminum oxide obtained has a purity of 95.3% and a high-quality ferrosilicon alloy with a Fe / Si ratio of 1.3.
[0053] Example 3
[0054] This embodiment provides a method for recovering iron and aluminum through direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation. The ore used in this embodiment is Ghanaian gibbsite-type high-iron bauxite, in which the useful mineral is gibbsite, and the gangue minerals are mainly aluminum goethite, hematite, kaolinite, rutile, quartz, etc., which contain Al by mass percentage. 2 O 3 48.9%, SiO 2 7.5%,Fe 2 O 3 31.2% and other inevitable impurities, belonging to gibbsite-type high-iron bauxite.
[0055] The specific steps are as follows:
[0056] The high-iron bauxite ore was crushed to a particle size of less than 1 cm by a jaw crusher, and the high-speed multifunctional pulverizer was finely ground to a particle size of less than 0.1 mm, accounting for 50% of the total weight; the reduced coal was finely ground to a particle size of less than 0.1 mm, accounting for 70% of the total weight, to obtain reduced coal powder. The high-iron bauxite and coal powder were put into a ball mill at a mass ratio of 100:6.7 and ground to a particle size of ≤0.074 mm, accounting for 70%, to obtain a mixture. The mixture was placed in a tubular furnace for reduction reaction, first evacuated to vacuum, and then nitrogen was introduced at a flow rate of 1.5L / min, and moderate direct reduction was carried out at 1300°C for 90 minutes to obtain reduced ore. The reduced ore is placed in a magnetic separator for the first stage of weak magnetic separation with a magnetic field strength of 150mT to obtain iron concentrate and aluminum concentrate, and carbon powder accounting for 5% of the total mass of the initial ore powder is spread on the surface and surrounding of the iron concentrate; the aluminum concentrate is subjected to the second stage of strong magnetic separation with a magnetic field strength of 1400mT; the iron concentrate and high-quality bauxite covered with coal powder are put into an arc smelting furnace and smelted at 2700℃ for 240min; after the smelting is completed, the copper crucible is cooled with the furnace, and the molten material is broken after cooling and solidification, and magnetic separation is carried out through a magnetic separation tube with a magnetic field strength of 160mT.
[0057] The final aluminum oxide obtained has a purity of 95.5% and a high-quality ferrosilicon alloy with a Fe / Si ratio of 1.4.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation, characterized in that: The specific steps include: S1. crushing and grinding high iron bauxite and reduced coal ore and mixing them evenly; S2, placing the mixture of high-iron bauxite and reduced coal into a tubular furnace filled with nitrogen for reduction; S3, performing weak magnetic separation on the reduced ore to screen out aluminum concentrate and iron concentrate, and spreading carbon powder on and around the surface of the iron concentrate; S4, conduct strong magnetic separation on aluminum concentrate to screen out high-quality bauxite and iron-aluminum spinel; S5, evenly mix the high-quality bauxite and the iron ore concentrate covered with reduced coal powder and put them into an electric arc furnace for smelting, and take them out after cooling after smelting; S6. The solidified lumps are broken up and magnetically separated by a magnetic separation device. After the magnetic separation, magnetic materials such as ferrosilicon alloy and high-purity alumina are obtained.
2. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S1, the high-iron bauxite is crushed to a particle size of less than 1 cm, and the portion finely ground to a particle size of less than 0.1 mm accounts for more than 50% of the total weight of the high-iron bauxite; the portion of the reduced coal finely ground to a particle size of less than 0.05 mm accounts for more than 70% of the total weight of the reduced coal.
3. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In the S1, the mass ratio of high iron bauxite to reduced coal is 100:2-10.
4. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S1, the high-iron bauxite is Ghanaian gibbsite-type high-iron bauxite, which includes Al2O3 45-55%, SiO2 5-10%, Fe2O3 30% and other inevitable impurities by mass percentage.
5. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S1, the reducing coal is lignite or anthracite.
6. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S2, direct reduction is carried out at 1100-1400°C for 60-180 min; the reduction is carried out until the ratio of the fixed carbon content in the reduced coal to the oxygen content of the iron oxide in the iron-containing mineral is 1-3, and the nitrogen flow rate is 1.5 L / min.
7. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S3, the magnetic field strength of weak magnetic separation is 90-160 mT, and the amount of carbon powder used is 5-10% of the amount of high-iron bauxite used in S1.
8. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In S4, the magnetic field strength is 1000-1600 mT.
9. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In the step S5, the smelting temperature is 2000-3000°C, and the smelting time is 180-360 minutes.
10. The method for recovering iron and aluminum by direct reduction of high-iron bauxite-electric furnace smelting-magnetic separation according to claim 1, characterized in that: In the S6, the magnetic field strength is 100-200 mT.
Citation Information
Patent Citations
Method for separating aluminum and iron in high-iron bauxite
CN101767057A
Iron-aluminum separation method for high-iron bauxite by proper reduction and sorting
CN102658235A
Method for comprehensively utilizing iron, aluminium and silicon in high-iron gibbsite
CN105177293A
Method for processing laterite nickel ore with direct production of ferronickel
WO2014133421A1
Cited By
Method for roasting and activating high-iron bauxite
CN120440918A
Method for resource utilization of high-iron and high-silicon bauxite
CN122012914A
Method for separating iron and aluminum by suspending and magnetizing roasting of high iron bauxite
CN123027418A