Low-carbon high-hole-expansion steel and preparation method thereof
By rationally designing the components and process flow in low-carbon high-strength steel, forming microstructures of ferrite, bainite and nano-precipitation phases, the problem of prone to cracking in the reaming process of high-strength steel is solved, and high-strength steel is achieved Preparation of low-carbon high-porous steel with strength and excellent pore reaming performance.
Patent Information
- Application Number
- CN202411176625.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-26
AI Technical Summary
High-strength steel is prone to cracking when making automotive parts with large hole expansion and large flange, and the existing high-strength steel has low tensile strength and lowered the surface quality of the steel plate.
The low-carbon design, reasonable composition and process flow, including hot rolling, cooling and coiling, improve the strength and pore reaming performance of the steel through the formation of nano-precipitation phases and specific microstructures. The specific steps include initial hot rolling, cooling, coiling of steel billets, and controlling the content of carbon, silicon and aluminum, adding trace amounts of Ti, Nb, V, Mo, and Cr microalloys, performing multiple hot rolling and cooling treatments to form ferrite , microstructure of bainite and nano-precipitated phases.
Low-carbon high-porous steel with yield strength greater than or equal to 650MPa, tensile strength greater than or equal to 800MPa, elongation greater than or equal to 20%, significantly improving the strength and porosity of the steel, while maintaining good surface quality. .
Smart Images

Figure CN118979190A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of advanced high hole expansion steel preparation, and in particular to a low carbon high hole expansion steel and a preparation method thereof. Background Art
[0002] With the rapid development of the automobile industry, people have higher and higher requirements for automobile safety, energy saving and emission, and the proportion of high-strength steel in the field of automobile parts is also increasing. However, it is found in the application process that high-strength steel has a high edge crack sensitivity and low hole expansion rate. It is easy to crack when making parts with large hole expansion and large flanging, which hinders the design and stamping technology of some parts. Therefore, more and more products require steel to have good hole expansion performance and extended flange properties while ensuring high strength.
[0003] In the related art, a high hole expansion steel plate and its manufacturing process are disclosed. Although a high hole expansion steel with a high hole expansion rate can be obtained, the corresponding tensile strength is low. In addition, in the process of preparing high hole expansion steel, a high content of Si is added to obtain steel with better performance, which will lead to a decrease in the surface quality of the steel plate; in addition, the high hole expansion steel prepared by the controlled rolling and controlled cooling process in the prior art generally has low strength. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to a certain extent, and provides a low-carbon high-hole expansion steel and a preparation method thereof.
[0005] As a first aspect of the present invention, a method for preparing low-carbon high-hole expansion steel is provided, comprising:
[0006] Providing initial steel billets;
[0007] Hot rolling the initial steel billet to obtain a hot-rolled plate, wherein the average equivalent circle diameter of the grains of the hot-rolled plate is between 2 μm and 5 μm, and the hot-rolled plate includes a nano-precipitated phase;
[0008] Cooling the hot-rolled plate to a coiling temperature to obtain a second steel plate, wherein the microstructure of the second steel plate includes ferrite, bainite and nano-precipitated phase;
[0009] The second steel plate is coiled and then cooled to obtain the low-carbon high hole expansion steel;
[0010] Wherein, the components of the initial steel billet include:
[0011]
[0012] Aluminum; silicon; the balance is Fe, and the composition of the initial steel billet satisfies the following relationship:
[0013] 0.12wt%≤WSi +W Al ≤0.35wt%;
[0014] Among them, W Si Indicates the silicon content, W Al Indicates the aluminum content.
[0015] Furthermore, in the step of hot rolling the initial steel billet, the initial steel billet is hot rolled for at least three passes, and the reduction ratios of the last two passes are between 60% and 70%.
[0016] Furthermore, in the step of performing multiple hot rolling on the initial steel billet, the starting rolling temperature is in the range of 1000° C. to 1030° C., the final rolling temperature is in the range of 850° C. to 890° C., and the total reduction ratio of hot rolling is between 90% and 95%.
[0017] Further, the hot-rolled plate is cooled to a coiling temperature to obtain a second steel plate, comprising:
[0018] Cooling at a first cooling rate to a ferrite transformation temperature range to obtain a first steel plate;
[0019] The first steel plate is cooled to a coiling temperature at a second cooling rate to obtain a second steel plate; wherein the first cooling rate is greater than the second cooling rate, and the coiling temperature is between 580°C and 620°C.
[0020] Further, in the step of cooling the hot-rolled plate to a ferrite transformation temperature range at a first cooling rate, the first cooling rate is between 30°C / s and 50°C / s, and the ferrite transformation temperature range is between 720°C and 750°C;
[0021] Furthermore, in the step of cooling the first steel plate to a set temperature at a second cooling rate, the second cooling rate is between 10° C. / s and 15° C. / s.
[0022] Furthermore, before cooling the first steel plate to a set temperature at a second cooling rate, the method further includes slowly cooling the first steel plate in air for 4 to 8 seconds.
[0023] Furthermore, in the step of cooling the second steel plate after coiling, the coiling temperature is in the range of 580° C. to 620° C., and cooling is performed in a heat preservation pit.
[0024] Furthermore, before hot rolling the initial steel billet, the preparation method further comprises:
[0025] Smelting the steel material into an ingot to obtain an ingot;
[0026] Forging the ingot to obtain a forged billet, wherein the final forging temperature is greater than or equal to 970° C.;
[0027] The forging billet is heated to a temperature between 1200° C. and 1260° C. and kept warm to obtain the initial billet, wherein the heating rate is between 150° C. / h and 200° C. / h and the keeping time is between 1.5h and 2h.
[0028] As a second aspect of the present invention, a low-carbon high-hole expansion steel is provided, and the low-carbon high-hole expansion steel is obtained by the above-mentioned preparation method.
[0029] Furthermore, the yield strength of the low-carbon high-hole expansion steel is greater than or equal to 650MPa, the tensile strength is greater than or equal to 800MPa, the elongation is greater than or equal to 20%, the hole expansion rate is greater than or equal to 75%, and the room temperature microstructure of the low-carbon high-hole expansion steel includes: α-ferrite, bainite and nano-precipitation phase.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) A more reasonable composition design is adopted to ensure better hole expansion performance while improving strength. Low carbon design C: 0.03-0.06%, carbon plays a role of solid solution strengthening in steel. In the present invention, the carbon content is guaranteed to be above 0.03% to obtain sufficient ferrite and higher strength. However, the carbon content cannot be higher than 0.06%, otherwise pearlite structure will be easily formed during hot rolling and coiling, which is not conducive to hole expansion performance. Therefore, the carbon content should be controlled between 0.03% and 0.06%, which can significantly improve the hole expansion rate and strength.
[0032] Low silicon aluminum design: ensure that the total content of Si and Al is between 0.12% and 0.35%. Si plays a role of solid solution strengthening in steel. Adding an appropriate amount can improve the strength, but with the increase of Si content, the surface quality of the steel decreases significantly. Controlling the Si content within a certain range ensures that the steel has better surface quality and strength. At the same time, Al will increase the complete austenitization temperature and expand the process window, but too much Al will lead to an increase in ferrite phase, which is not conducive to strength improvement. Therefore, controlling the total content of Si and Al between 0.12% and 0.35% is ideal for improving steel performance.
[0033] At the same time, by adding trace amounts of Ti, Nb, V, Mo, and Cr microalloys, a nano-carbide phase of (Ti, Nb, V, Mo, Cr) is compositely precipitated during the rolling, cooling, and coiling processes, which has the effect of fine grain and precipitation strengthening.
[0034] (2) The use of a low temperature and high reduction rate hot rolling process can not only increase the accumulation of dislocations to provide strength, but also produce sufficient deformation to refine the grains. At the same time, strain-induced nano-precipitation phases can be obtained. The nano-precipitation phases can hinder the further growth of the grains. The nano-precipitation phases are evenly distributed in the organization. The grains are broken and homogenized under the action of rolling force and nano-precipitation phases, avoiding the existence of too many mixed crystals, reducing stress concentration during subsequent strain or hole expansion deformation, and preventing premature crack initiation. The microstructure of the hot-rolled plate after hot rolling has small and uniform grain size, the presence of nano-precipitation phases, and high dislocation density, which creates a precursor microstructure with fine grains, nano-precipitation phases and high dislocation density for the subsequent preparation process.
[0035] (3) The cooling and coiling process is used to further optimize the microstructure of the hot-rolled plate in the previous step by heat treatment, creating a two-phase microstructure of ferrite and bainite in a specific ratio. At the same time, more nano-precipitates are precipitated to play a strengthening role. Through the combination of ferrite, bainite and nano-precipitates, low-carbon high-hole expansion steel with better strength, plasticity and hole expansion is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0037] Figure 1 It is a flow chart of an implementation method of the method for preparing low-carbon high-hole expansion steel provided by the present invention;
[0038] Figure 2 is a flow chart of an implementation method of the second steel plate provided by the present invention;
[0039] Figure 3 It is a flow chart of another embodiment of the method for preparing low-carbon high hole expansion steel provided by the present invention;
[0040] Figure 4 It is a flow chart of an implementation method of the method for preparing the initial steel billet provided by the present invention;
[0041] Figure 5 is a scanning electron microscope photograph of the microstructure of Example 1 of the present invention;
[0042] Figure 6 is a transmission electron microscope photograph of the nano-precipitate phase distribution of Example 1 of the present invention;
[0043] Figure 7This is an electron backscatter diffraction (EBSD) image of the hole expansion crack in Example 1 of the present invention.
[0044] Reference numerals
[0045] 1: Ferrite
[0046] 2: Bainite
[0047] 3: Nano-precipitation phase
[0048] 4: Hole expansion crack DETAILED DESCRIPTION
[0049] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.
[0050] References to "one embodiment" or "example" or "example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed herein. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.
[0051] As a first aspect of the present invention, a flow chart of an implementation method of a method for preparing low-carbon high-hole expansion steel is provided, such as Figure 1 As shown, including:
[0052] In step S110, an initial steel billet is provided;
[0053] In step S120, the initial steel billet is hot rolled to obtain a hot rolled plate, the average equivalent circle diameter of the grains of the hot rolled plate is between 2 μm and 5 μm, and the hot rolled plate includes a nano-precipitated phase;
[0054] In step S130, the hot-rolled plate is cooled to a coiling temperature to obtain a second steel plate, wherein the microstructure of the second steel plate includes ferrite, bainite and nano-precipitated phases;
[0055] In step S140, the second steel plate is coiled and then cooled to obtain low-carbon high-hole expansion steel;
[0056] Among them, the components of the initial steel billet include:
[0057] Carbon 0.03-0.06wt%;
[0058] Manganese 1.55-1.8wt%;
[0059] Chromium 0.55-0.8wt%;
[0060] Titanium 0.08-0.10wt%;
[0061] Niobium 0.02-0.05wt%;
[0062] Vanadium 0.02-0.06wt%;
[0063] Molybdenum 0.02-0.05wt%;
[0064] Aluminum; Silicon; the balance is Fe, and the composition of the initial steel billet satisfies the following relationship:
[0065] 0.12wt%≤W Si +W Al ≤0.35wt%;
[0066] Among them, W Si Indicates the silicon content, W Al Indicates the aluminum content.
[0067] In step S110, an initial steel billet with component design is used to improve strength while ensuring better hole expansion performance. Low carbon design C: 0.03-0.06%, carbon plays a role of solid solution strengthening in steel. In the present invention, the carbon content is guaranteed to be above 0.03% to obtain a sufficient amount of ferrite and higher strength. However, the carbon content cannot be higher than 0.06%, otherwise pearlite structure will be easily formed during hot rolling and coiling, which is not conducive to hole expansion performance. Therefore, the carbon content should be controlled between 0.03% and 0.06%, which can significantly improve the hole expansion rate and strength.
[0068] Low silicon aluminum design: ensure that the total content of Si and Al is between 0.12% and 0.35%. Si plays a role of solid solution strengthening in steel. Adding an appropriate amount can improve the strength, but with the increase of Si content, the surface quality of the steel decreases significantly. Controlling the Si content within a certain range ensures that the steel has better surface quality and strength. At the same time, Al will increase the complete austenitization temperature and expand the process window, but too much Al will lead to an increase in the ferrite phase, which is not conducive to strength improvement. Therefore, controlling the total content of Si and Al between 0.12% and 0.35% is ideal for improving steel performance.
[0069] At the same time, by adding trace amounts of Ti, Nb, V, Mo, and Cr microalloys, a nano-carbide phase of (Ti, Nb, V, Mo, Cr) is compositely precipitated during the rolling, cooling, and coiling processes, which has the effects of fine grain strengthening and precipitation strengthening.
[0070] In step S120, a hot rolling process with a relatively low temperature and a large reduction rate is adopted, which can not only increase more dislocation accumulation to provide strength, but also produce sufficient deformation to refine the grains, and at the same time ensure that the grains are broken and uniformly formed under the rolling force and the composite nano-precipitation, avoid the existence of too many mixed crystals, reduce stress concentration in the subsequent strain or hole expansion deformation process, and prevent the premature initiation of cracks. The hot-rolled plate has a small and uniform grain size after hot rolling, with an average equivalent circular diameter of 2μm to 5μm, a high dislocation density, and a strain-induced precipitation nano-precipitation phase, which creates an ideal precursor microstructure for the subsequent preparation process.
[0071] As an optional embodiment, in the step of hot rolling the initial steel billet, the initial steel billet is hot rolled for at least 3 passes, preferably, the total number of hot rolling passes includes 5 passes, and the reduction rate of the last two passes is between 60% and 70%. The hot rolling temperature of the last two passes is relatively lower, but the reduction rate is relatively higher. The use of such a large reduction rate at a lower temperature can not only further increase more dislocation accumulation to provide strength, but also ensure that the grains are further broken and homogenized under the action of rolling force and composite nano precipitation, avoid the existence of more mixed crystals, reduce stress concentration in subsequent strain or hole expansion deformation, and prevent premature crack initiation.
[0072] As an optional implementation, the hot rolling start temperature is in the range of 1000° C. to 1030° C., and the hot rolling start temperature is carried out in the full austenite temperature range. Multiple hot rolling can fully refine the original austenite grain size.
[0073] As an optional implementation, the final rolling temperature of hot rolling is in the range of 850°C to 890°C. The gradual decrease in the hot rolling temperature will, on the one hand, phase transform a small part of α ferrite, and on the other hand, hot rolling within this temperature will also strain-induce the precipitation of a large amount of micro-metal carbides. The precipitated carbides can further refine the grains and have the effect of precipitation strengthening. In addition, the lower warm rolling temperature and greater reduction rate ensure more dislocation accumulation, creating a precursor for fine-grained, precipitated and high-density dislocation structure and being inherited by subsequent hot forming processes.
[0074] As an optional embodiment, the total reduction rate of hot rolling is between 90% and 95%, which can enable the initial steel billet to be fully deformed in the hot rolling stage, fully refine the original austenite grain size in the steel billet, and have a sufficiently high dislocation stacking, and the average equivalent circular diameter of the grains after hot rolling is between 2μm and 5μm.
[0075] In step S130 and step S140, the hot-rolled plate is cooled to the coiling temperature to obtain a second steel plate, the microstructure of which includes ferrite, bainite and nano-precipitated phase; the second steel plate is then coiled and cooled to obtain a low-carbon high-hole expansion steel.
[0076] The cooling and coiling process is used to further optimize the structure of the hot-rolled plate in the previous step through heat treatment, creating a two-phase structure of ferrite and bainite in a specific proportion. At the same time, more nano-precipitates are precipitated to play a strengthening role. Through the combination of ferrite, bainite and nano-precipitates, low-carbon, high-hole-expansion steel with better strength, plasticity and hole expansion can be obtained.
[0077] As an optional implementation, Figure 2 As shown, the hot rolled plate is cooled to a coiling temperature to obtain a second steel plate, comprising:
[0078] In step S131, cooling to a ferrite transformation temperature range at a first cooling rate to obtain a first steel plate;
[0079] In step S132, the first steel plate is cooled to a coiling temperature at a second cooling rate to obtain a second steel plate, wherein the first cooling rate is greater than the second cooling rate, and the coiling temperature is between 580°C and 620°C.
[0080] In step S131, the hot-rolled plate is cooled to a ferrite transformation temperature range at a first cooling rate. The first cooling rate is relatively fast. On the one hand, it ensures the growth of sufficient ferrite to create a pre-organization basis for a two-phase structure of ferrite and bainite in a certain proportion. On the other hand, it further causes the composite precipitation of microalloys and carbides to achieve the effect of precipitation strengthening. As an optional implementation, the first cooling rate is between 30°C / s and 50°C / s, and the ferrite transformation temperature range is between 720°C and 750°C.
[0081] In step S132, the first steel plate is cooled to the coiling temperature at a second cooling rate to obtain a second steel plate. The second cooling rate is relatively slow, ensuring that a sufficient proportion of ferrite and bainite are formed within the common transformation range of ferrite and bainite, and together with the first cooling stage, a two-phase structure of ferrite and bainite of a certain proportion is created, while also ensuring a sufficient amount of microalloy precipitation and carbide precipitation to further play a strengthening role.
[0082] In step S131, the coiling temperature is between 580°C and 620°C. A relatively high coiling temperature is used to ensure the combined precipitation of various microalloy carbides and the combined effect of grain recovery and recrystallization, promote precipitation strengthening and the interaction between precipitation and dislocation.
[0083] As an optional implementation, the second cooling rate is between 10°C / s and 15°C / s.
[0084] As an optional implementation, after the first cooling stage, the first steel plate is slowly cooled in air for 4 to 8 seconds and then cooled for a second time.
[0085] As an optional implementation, the second steel plate coiling temperature is in the range of 580°C to 620°C, the coiled steel strip is placed in an insulation pit for insulation and slow cooling, and is taken out after 24 hours to obtain low-carbon high-hole expansion steel.
[0086] like Figure 3 As shown, the present invention provides a flow chart of an embodiment of a method for preparing low-carbon high-hole expansion steel, wherein the preparation method comprises:
[0087] In step S210, an initial steel billet is provided;
[0088] In step S220, the initial steel billet is hot-rolled for at least three passes, and the reduction ratio of the last two passes is between 60% and 70%, to obtain a hot-rolled plate;
[0089] In step S230, the hot-rolled plate is cooled to a temperature range of 720°C to 750°C at a cooling rate between 30°C / s and 50°C / s to obtain a first steel plate;
[0090] In step S240, the first steel plate is cooled to a temperature in the range of 580°C to 620°C at a cooling rate between 10°C / s and 15°C / s to obtain a second steel plate;
[0091] In step S250, the second steel plate is coiled and placed in a heat preservation pit for slow cooling, and is taken out after 24 hours to obtain low-carbon high-hole expansion steel.
[0092] In the embodiment of the present invention, there is no particular limitation on how to obtain the initial steel billet. For example, the initial steel billet can be obtained by purchasing from outside. For another example, the initial steel billet can be obtained directly by smelting, calcining and heat treating steel.
[0093] As an optional implementation, Figure 4 As shown, before hot rolling the initial steel billet, the preparation method further includes:
[0094] In step S111, the steel material is smelted and cast into an ingot to obtain a steel ingot;
[0095] In step S112, the steel ingot is heated to a temperature between 1150°C and 1250°C and kept warm to obtain a first steel ingot, wherein the heating rate is between 150°C / h and 200°C / h and the holding time is between 2.6h and 3.6h. This step is a conventional homogenization process;
[0096] In step S113, the first steel ingot is forged to obtain a forged billet, wherein the final forging temperature is greater than or equal to 960° C.;
[0097] In step S114, the forging billet is heated to a temperature between 1150°C and 1250°C and kept warm to obtain the initial billet, wherein the heating rate is between 200°C / h and 300°C / h and the keeping time is between 1.6h and 2.6h.
[0098] The process route of the invention is simple, and the heat treatment cycle is greatly shortened, which is conducive to achieving low-cost and high-efficiency production.
[0099] The low-carbon high hole expansion steel in the present invention adopts the initial steel billet designed with the above components and is obtained by the above preparation method. The low-carbon high hole expansion steel has a tensile strength greater than or equal to 800 MPa, a yield strength greater than or equal to 650 MPa, an elongation greater than or equal to 20.0%, and a hole expansion rate greater than or equal to 75%. The room temperature microstructure of the obtained low-carbon high hole expansion steel includes α ferrite, bainite and nano-precipitation phase.
[0100] The present invention will be further described below through specific examples and comparative examples.
[0101] Example
[0102] In the following embodiments of the present invention, the components of the steel billet used are as follows:
[0103]
[0104]
[0105] Aluminum; Silicon; the balance is Fe, and the composition of the initial steel billet satisfies the following relationship:
[0106] W Si +W Al 0.26wt%;
[0107] Among them, W Si Indicates the silicon content, W Al Indicates the aluminum content.
[0108] Example 1
[0109] A low-carbon high-hole expansion steel and a preparation method thereof, comprising:
[0110] The first step: smelting the steel billet to obtain a cast billet;
[0111] Step 2: Forging the ingot to obtain a forged ingot, wherein the final forging temperature is maintained to be greater than or equal to 970°C;
[0112] Step 3: The forging billet is heated to 1200°C at a heating rate of 200°C / h and kept at this temperature for 1.8h to obtain an initial billet;
[0113] Step 4: hot rolling the initial steel billet to obtain a hot rolled plate, wherein the hot rolling start temperature is 1000°C, the final rolling temperature is 870°C, the total reduction rate of the hot rolling 5 passes is 92%, and the cumulative reduction rate of the last two passes is 60%;
[0114] Step 5: Cool the hot rolled plate to 750°C at a cooling rate of 45°C / s, slowly cool in air for 4s and then cool to 600°C at a cooling rate of 15°C / s;
[0115] Step 6: Coil the hot-rolled plate after cooling in the previous step at a coiling temperature of 600°C. Put the coiled steel strip into a heat preservation pit for slow cooling and take it out after 24 hours to obtain sample 1.
[0116] Microstructure Figure 5 As shown, the room temperature structure contains about 40% ferrite and about 60% bainite by volume, and the nano-second phase precipitation is as follows Figure 6 As shown, the EBSD image of the hole expansion crack is as follows Figure 7 Other relevant process parameters and mechanical properties are shown in Tables 1 and 2.
[0117] Example 2
[0118] 800MPa grade low carbon high hole expansion steel was prepared by the method provided in Example 1, except that the total reduction rate of the last two passes of the hot rolling process in Example 2 was 68%, the coiling temperature was 620°C, and sample 2 was obtained. The specific process parameters are shown in Table 1.
[0119] Example 3
[0120] 800MPa grade low carbon high hole expansion steel was prepared by the method provided in Example 1, except that in the cooling process of Example 3, the hot rolled plate was first cooled to 725°C at a cooling rate of 30°C / s, slowly cooled in air for 7s and then cooled to 580°C at a cooling rate of 10°C / s to obtain Sample 3. The specific process parameters are shown in Table 1.
[0121] Comparative Example 1
[0122] 800MPa grade low carbon high hole expansion steel was prepared by the method provided in Example 1, except that the total reduction rate of the last two passes of the hot rolling process of Example 1 was 40%, and sample 4 was obtained. The specific process parameters are shown in Table 1.
[0123] Comparative Example 2
[0124] 800MPa grade low carbon high hole expansion steel was prepared by the method provided in Example 1, except that, in the cooling process of Example 2, the hot rolled plate was cooled to 600°C at a cooling rate of 45°C / s in the cooling process to obtain Sample 5. The specific process parameters are shown in Table 1.
[0125] Comparative Example 3
[0126] 800 MPa grade low carbon high hole expansion steel was prepared by the method provided in Example 1, except that the coiling temperature of Comparative Example 3 was 450°C, and Sample 6 was obtained. The specific process parameters are shown in Table 1.
[0127] Test Case
[0128] The microstructure of sample 1 was obtained using a Zeiss Gemini SEM 500 scanning electron microscope. Figure 5 As shown; the nano-precipitation phase distribution photo of sample 1 was obtained using a transmission electron microscope FEI F20, as shown Figure 6 As shown; the expansion crack growth photo of sample 1 was obtained by electron backscatter diffraction Symmetry S2, as shown Figure 7 The mechanical properties and hole expansion ratio of the samples were tested using a universal testing machine (MTS E45.305), and the test data are shown in Table 2.
[0129] Figure 5 and Figure 6 It is shown that the microstructure of sample 1 includes ferrite 1, bainite 2 and nano-precipitates 3, specifically including about 40% ferrite + 60% bainite + nano-precipitates. Figure 7 It shows that the grains around the hole expansion crack 4 of sample 1 are evenly distributed and small, which effectively hinders the further expansion of the crack and improves the hole expansion performance of sample 1. Sample 1 has a yield strength of 670MPa, a tensile strength of 825MPa, an elongation of 20.5%, and a hole expansion rate of 78%.
[0130] Sample 2 increases the total reduction rate of the last two hot rolling passes from 60% reduction rate in Example 1 to 68% in Example 2, and slightly increases the coiling temperature. The microstructure is the same as that of Sample 1, which is ferrite and bainite. Due to the increase in reduction rate, the grains of Sample 2 are further refined and the mechanical properties are improved. Sample 2 has a yield strength of 702MPa, a tensile strength of 844MPa, an elongation of 21.2%, and a hole expansion rate of 75%.
[0131] Sample 3 reduces the cooling rate and the final temperature of the two coolings. The lower cooling rate gives the ferrite structure more time to form and grow, but also reduces the coiling temperature. The ferrite and bainite contents are basically the same as those of Sample 1. The yield strength of Sample 3 is 656MPa, the tensile strength is 820MPa, the elongation is 20.9%, and the hole expansion rate is 77%.
[0132] Sample 4 reduces the total reduction rate of the last two hot rolling passes, from 60% reduction rate in Example 1 to 40% in Comparative Example 1, and the deformation is insufficient. The microstructure of Sample 4 includes about 40% ferrite + 60% bainite + nano-precipitation phase, less dislocation accumulation, more mixed crystals, insufficient dislocation accumulation, grain refinement and homogenization, and significantly reduced mechanical properties. Sample 4 has a yield strength of 645 MPa, a tensile strength of 799 MPa, an elongation of 18.7%, and a hole expansion rate of 65%;
[0133] Sample 5 is directly cooled to the coiling temperature at the first cooling rate. It does not transform and form enough ferrite in the cooling stage, resulting in a decrease in the ferrite content and excessive bainite content. Bainite is a hard phase, which is not conducive to hole expansion performance and a low hole expansion rate. The microstructure of Sample 5 includes about 33% ferrite + 67% bainite + nano-precipitate phase. The yield strength of Sample 5 is 724MPa, the tensile strength is 857MPa, the elongation is 16.4%, and the hole expansion rate is 40%;
[0134] When the coiling temperature of Sample 6 is reduced to 450°C, the bainite content further increases. However, the lower temperature significantly reduces the content of nano-precipitation phase, and the precipitation size is larger, and the mechanical properties and hole expansion properties are poor. The microstructure of Sample 6 includes about 27% ferrite + 73% bainite, with less precipitation or large precipitation size. The yield strength of Sample 6 is 685MPa, the tensile strength is 760MPa, the elongation is 20.0%, and the hole expansion rate is 46%.
[0135] Table 1 Process parameters of the embodiments of the present invention and the comparative examples
[0136]
[0137] Table 2 Mechanical properties and microstructure of the embodiments of the present invention and the comparative examples
[0138]
[0139] It can be seen from Tables 1 and 2 that the component design and preparation method of the present invention can be used to obtain low-carbon high hole expansion steel with better comprehensive performance in strength, elongation and hole expansion rate. Multiple hot rolling with large deformation, combined with multi-stage cooling with different cooling rates and appropriate coiling temperature, make the low-carbon high hole expansion steel of the present invention have an ideal and appropriate proportion of ferrite, bainite and nano-precipitation phase, and sufficient dislocation accumulation and grain refinement, so as to obtain better performance.
[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing low-carbon high-hole expansion steel, It is characterized in that include: Providing initial steel billets; Hot rolling the initial steel billet to obtain a hot-rolled plate, wherein the average equivalent circle diameter of the grains of the hot-rolled plate is between 2 μm and 5 μm, and the hot-rolled plate includes a nano-precipitated phase; Cooling the hot-rolled plate to a coiling temperature to obtain a second steel plate, wherein the microstructure of the second steel plate includes ferrite, bainite and nano-precipitated phase; The second steel plate is coiled and then cooled to obtain the low-carbon high hole expansion steel; Wherein, the components of the initial steel billet include: Aluminum; silicon; the balance is Fe, and the composition of the initial steel billet satisfies the following relationship: 0.12wt%≤W Si +W Al ≤0.35wt%; Among them, W Si Indicates the silicon content, W Al Indicates the aluminum content.
2. The preparation method according to claim 1, It is characterized in that In the step of hot rolling the initial steel slab, the initial steel slab is hot rolled for at least three passes, and the reduction ratios of the last two passes are between 60% and 70%.
3. The preparation method according to claim 2, It is characterized in that In the step of hot rolling the initial steel billet for multiple times, the starting rolling temperature is in the range of 1000° C. to 1030° C., the final rolling temperature is in the range of 850° C. to 890° C., and the total reduction ratio of hot rolling is between 90% and 95%.
4. The preparation method according to claim 1, It is characterized in that Cooling the hot-rolled plate to a coiling temperature to obtain a second steel plate, comprising: Cooling at a first cooling rate to a ferrite transformation temperature range to obtain a first steel plate; The first steel plate is cooled to a coiling temperature at a second cooling rate to obtain a second steel plate; wherein the first cooling rate is greater than the second cooling rate, and the coiling temperature is between 580°C and 620°C.
5. The preparation method according to claim 4, It is characterized in that In the step of cooling the hot-rolled plate to a ferrite transformation temperature range at a first cooling rate, the first cooling rate is between 30°C / s and 50°C / s, and the ferrite transformation temperature range is between 720°C and 750°C.
6. The preparation method according to claim 4, It is characterized in that In the step of cooling the first steel plate to a set temperature at a second cooling rate, the second cooling rate is between 10° C. / s and 15° C. / s.
7. The preparation method according to claim 6, It is characterized in that Before cooling the first steel plate to a set temperature at a second cooling rate, the method further includes slowly cooling the first steel plate in air for 4 to 8 seconds.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that Before hot rolling the initial steel billet, the preparation method further comprises: Smelting the steel material into an ingot to obtain an ingot; Forging the ingot to obtain a forged billet, wherein the final forging temperature is greater than or equal to 970° C.; The forging billet is heated to a temperature between 1200° C. and 1260° C. and kept warm to obtain the initial billet, wherein the heating rate is between 150° C. / h and 200° C. / h and the keeping time is between 1.5h and 2h.
9. A low carbon high hole expansion steel, It is characterized in that The low-carbon high-hole expansion steel is obtained by the preparation method described in any one of claims 1 to 8.
10. The low carbon high hole expansion steel according to claim 9, It is characterized in that The yield strength of the low-carbon high-hole expansion steel is greater than or equal to 650MPa, the tensile strength is greater than or equal to 800MPa, the elongation is greater than or equal to 20%, and the hole expansion rate is greater than or equal to 75%. The room temperature microstructure of the low-carbon high-hole expansion steel includes: α-ferrite, bainite and nano-precipitation phase.
Citation Information
Patent Citations
Low-carbon hot-rolled full-ferrite based steel with ultrahigh strength and ultrahigh reaming ratio and preparation method thereof
CN103194675A
980 MPa-grade hot-rolled ferritic bainite high-reaming dual-phase steel and manufacturing method thereof
CN105925888A
980MPa-grade cold rolled steel plate with high reaming rate and higher elongation and manufacturing method thereof
CN109576579A
980 mpa-grade bainite high hole expansion steel and manufacturing method therefor
US20230313333A1
1000mpa-grade high hole expansion hot-rolled complex phase steel plate and manufacturing method thereof
WO2023241545A1
Cited By
High-strength wheel steel and preparation method thereof
CN119979846A