Structural steel capable of eliminating watermarks on surface of steel plate and used for engineering machinery and production method of structural steel

By controlling the chemical composition of Si, Ti, Mn and N and adopting air-cooling technology, the watermark problem on the surface of the steel plate is solved, the appearance quality and mechanical properties are improved, the needs of engineering machinery are met, and the production costs are reduced.

CN118979192APending Publication Date: 2024-11-19NANJING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411030791.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the production process of structural steel for construction machinery, the controlled rolling and cooling process causes watermarks to appear on the surface of the steel plate, affecting the appearance and use requirements, and it is difficult to completely eliminate the watermark color difference problem during subsequent processing.

Method used

By controlling the chemical composition content of Si, Ti, Mn and N in the molten iron, the formation of FeSiO4 iron oxide is reduced, and the air-cooling process is used instead of the cooling control process, combined with a reasonable rolling process, the grain size is refined and the microstructure is optimized to avoid The generation of watermarks.

Benefits of technology

It realizes smooth and uniform appearance quality on the surface of the steel plate, improves the mechanical properties and bending properties of the materials, meets the use needs of different construction machinery, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979192A_ABST
    Figure CN118979192A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of structural steel, in particular to structural steel for engineering machinery and capable of eliminating watermarks on the surface of a steel plate and a production method of the structural steel, and the structural steel comprises the following chemical components in percentage by mass: 0.14-0.18% of C, 1.10-1.20% of Mn, less than or equal to 0.20% of Si, 0.040-0.050% of Ti, less than or equal to 0.020% of P, less than or equal to 0.005% of S, less than or equal to 0.00005% of N and the balance of iron and inevitable impurities. By accurately controlling the contents of chemical components of Si, Ti, Mn and N in molten iron, FeSiO4-containing oxide scales which are difficult to eliminate are reduced, watermarks which are difficult to eliminate are prevented from being formed in the hot rolling process of the steel plate, meanwhile, an air cooling process is adopted in a matched mode, the generation of the watermarks on the surface of the steel plate is further prevented, the surface of the steel plate is smoother and more uniform through the combined synergistic effect of the two, and the quality of the steel plate is improved. And defects are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of structural steel for engineering machinery, in particular to structural steel for engineering machinery capable of eliminating watermarks on the surface of steel plates and a production method thereof. Background Art

[0002] With the rapid development of my country's social economy, the requirements for steel quality in engineering projects are getting higher and higher, especially the demand for high-strength structural steel is growing. The 355MPa grade structural steel produced by medium and thick plate enterprises has good application prospects in engineering applications. However, in the current production process, in order to reduce costs, most companies adopt controlled rolling and controlled cooling technology, which leads to watermarks on the surface of the steel plate after water cooling, affecting the appearance and use requirements. In the subsequent processing process, shot blasting and painting procedures are also difficult to eliminate the color difference of watermarks on the surface of the steel plate, affecting the appearance and use requirements. For this reason, this application proposes a structural steel for engineering machinery that eliminates watermarks on the surface of steel plates and a production method thereof. Summary of the invention

[0003] The present invention aims at solving the above-mentioned technical problems, overcomes the shortcomings of the prior art, and provides a structural steel for engineering machinery and a production method thereof for eliminating watermarks on the surface of steel plates, thereby reducing the difficult-to-eliminate iron oxide scale containing FeSiO4 and avoiding the formation of difficult-to-eliminate watermarks on steel plates during hot rolling.

[0004] In the first aspect, the structural steel for engineering machinery for eliminating watermarks on the surface of steel plates provided by the present invention has the following chemical composition and mass percentage: C: 0.14-0.18, Mn: 1.10-1.20, Si: ≤0.20, Ti: 0.040-0.050, P: ≤0.020, S: ≤0.005, N: ≤0.00005, and the remainder is iron and unavoidable impurities.

[0005] Furthermore, the chemical composition and mass percentage of the structural steel for engineering machinery are as follows: C: 0.15-0.17, Mn: 1.10-1.20, Si: ≤0.20, Ti: 0.040-0.050, P: ≤0.020, S: ≤0.005, N: ≤0.00005, and the remainder is iron and unavoidable impurities.

[0006] It should be noted that the present application controls the Si content below 0.20%, which can reduce the difficult-to-eliminate iron oxide scale containing FeSiO4 (fayalite), which will easily form difficult-to-eliminate watermarks during the hot rolling process. By adding 0.040-0.050% Ti, the mechanical properties of the steel plate are improved by utilizing its strong precipitation and precipitation strengthening effects to offset the performance degradation after reducing the Mn content (from the conventional 1.40-1.50% to 1.10-1.20%). The price difference between Ti and Mn alloys is utilized to achieve the purpose of reducing production costs. Furthermore, by controlling the low N element to form large particles of TiN, stress concentration can be reduced and the risk of cracking can be reduced, thereby improving the bending performance of the steel plate.

[0007] In a second aspect, the present invention also provides a method for producing structural steel for engineering machinery, which specifically comprises the following steps:

[0008] Converter smelting: add scrap steel and molten iron, and then add slag making materials in batches;

[0009] Refining: deoxidation and alloying, RH vacuum treatment, calcium treatment after vacuum, static stirring;

[0010] Continuous casting: Vertical bending continuous casting is used for casting, and conventional rolling is carried out after the billet is piled up for cold surface inspection.

[0011] Furthermore, the content in molten iron is controlled as follows: Si: ≤0.20, Ti: 0.040-0.050, Mn: 1.10-1.20.

[0012] Furthermore, in the rolling process, the thickness of the warm billet is set to be ≥2.0 times to ensure the reduction amount of the finishing pass, and the grain size of the structure is refined by rolling to improve the strength and toughness of the material.

[0013] Furthermore, in the rolling process, the final rolling temperature is controlled below 820° C. to prevent coarsening of grains and avoid affecting the performance of the steel.

[0014] Furthermore, the steel plate is air-cooled after rolling. The air-cooling process has a more uniform cooling rate, reduces the unevenness of cooling, prevents the watermark problem on the surface of the steel plate caused by the controlled cooling process, and improves the appearance quality of the product.

[0015] By controlling the above chemical composition and production process, a microstructure with fine and uniform grains can be obtained, which helps to improve the overall performance of the material.

[0016] The beneficial effects of the present invention are:

[0017] (1) The present invention controls the Si content below 0.20% by precisely controlling the chemical composition contents of Si, Ti, Mn and N in the molten iron, thereby reducing the hard-to-eliminate iron oxide scale containing FeSiO4 and avoiding the formation of hard-to-eliminate watermarks on the steel plate during the hot rolling process. At the same time, the air cooling process is used instead of the controlled cooling process to further prevent the formation of watermarks on the surface of the steel plate. The combined synergistic effect of the two makes the surface of the steel plate smoother and more uniform, reduces defects, and improves the appearance quality of the product;

[0018] (2) The present invention utilizes the precipitation strengthening effect of titanium by adding Ti and Mn in a reasonable ratio. Even when the manganese content is reduced, the mechanical properties of the steel plate are improved by utilizing its strong precipitation and precipitation strengthening effects. The low nitrogen content is controlled to form large particles of TiN, which reduces stress concentration, reduces crack risks, and improves the bending performance of the steel plate.

[0019] (3) The present invention achieves a fine and uniform grain microstructure by controlling the chemical composition and rolling process, which helps to improve the overall performance of the material. By refining the grain size and optimizing the microstructure, the adaptability of the material is improved, enabling it to meet the use requirements of different engineering machinery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The metallographic structure diagram of the steel plate surface in Example 1 of the present invention;

[0021] Figure 2 This is a physical picture of the steel plate in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The solution provided in this application is mainly used for structural steel plates for engineering machinery produced by medium and thick plate enterprises. It solves the watermark problem on the surface of the steel plates, which can not only improve the surface quality of the steel plates, solve the watermark problem, and meet the user's requirements for a scratch-free process, but also reduce production costs and improve economic benefits.

[0023] As an optional implementation mode of the present invention, the chemical composition and mass percentage of structural steel for engineering machinery for eliminating watermarks on the surface of steel plates are as follows: C: 0.14-0.18, Mn: 1.10-1.20, Si: ≤0.20, Ti: 0.040-0.050, P: ≤0.020, S: ≤0.005, N: ≤0.00005, and the remainder is iron and unavoidable impurities.

[0024] At the same time, corresponding to the above-mentioned embodiment, the production method of structural steel for engineering machinery includes the following steps:

[0025] Converter smelting: add scrap steel and molten iron, and then add slag making materials in batches;

[0026] Refining: deoxidation and alloying, RH vacuum treatment, calcium treatment after vacuum, static stirring, control the content of molten iron: Si: ≤0.20, Ti: 0.040-0.050, Mn: 1.10-1.20, post-calcium treatment and then vacuum treatment;

[0027] Continuous casting: vertical bending continuous casting is adopted for casting, and conventional rolling is carried out after the billet is piled and cooled and inspected. In the rolling process, the thickness of the warm billet is set to ≥2.0 times to ensure the reduction of the finishing pass, the final rolling temperature is controlled below 820°C, and the steel plate is air-cooled after rolling.

[0028] This is demonstrated below through two specific embodiments.

[0029] Table 1 Chemical composition of each embodiment of the present application (wt%)

[0030] Example C,% Mn, % Si, % P,% S,% Ti, % N, ppm Example 1 0.15 1.17 0.17 0.014 0.004 0.045 24 Example 2 0.17 1.15 0.20 0.016 0.003 0.049 27

[0031] Embodiment 1:

[0032] Product number: 2420582102, steel type: Q355B, final rolling temperature 819℃, air cooling. Performance test results: yield strength 382MPa, tensile strength 499MPa, elongation 25%, 20℃ impact energy 275J. Surface test results: no watermark.

[0033] Embodiment 2:

[0034] Product number: 2410584301, steel type: Q355B, final rolling temperature 817℃, air cooling. Performance test results: yield strength 397MPa, tensile strength 536MPa, elongation 27.5%, impact energy at 20℃ 218J. Surface test results: no watermark.

[0035] In summary, the present application achieves a fine and uniform grain microstructure by controlling the chemical composition and rolling process, which helps to improve the overall performance of the material, control the Si content below 0.20%, reduce the difficult-to-eliminate iron oxide scale containing FeSiO4, and avoid the formation of difficult-to-eliminate watermarks on the steel plate during the hot rolling process. By refining the grain size and optimizing the microstructure, the adaptability of the material is improved, enabling it to meet the use requirements of different engineering machinery. The use of air cooling technology instead of the controlled cooling process further effectively prevents the formation of watermarks on the steel plate surface and improves the appearance quality of the product.

[0036] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A structural steel for engineering machinery for eliminating watermarks on the surface of steel plates, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.14-0.18, Mn: 1.10-1.20, Si: ≤0.20, Ti: 0.040-0.050, P: ≤0.020, S: ≤0.005, N: ≤0.00005, and the balance is iron and unavoidable impurities.

2. The structural steel for construction machinery according to claim 1, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.15-0.17, Mn: 1.10-1.20, Si: ≤0.20, Ti: 0.040-0.050, P: ≤0.020, S: ≤0.005, N: ≤0.00005, and the balance is iron and unavoidable impurities.

3. A method for producing structural steel for engineering machinery according to claim 1 or 2, characterized in that: The following steps are involved: Converter smelting: add scrap steel and molten iron, and then add slag making materials in batches; Refining: deoxidation and alloying, RH vacuum treatment, calcium treatment after vacuum, static stirring; Continuous casting: Vertical bending continuous casting is used for casting, and conventional rolling is carried out after the billet is piled up for cold surface inspection.

4. The method for producing structural steel for construction machinery according to claim 3, characterized in that: Control the content in molten iron: Si: ≤0.20, Ti: 0.040-0.050, Mn: 1.10-1.

20.

5. The method for producing structural steel for construction machinery according to claim 3, characterized in that: In the rolling process, the thickness of the warm billet is set to be ≥2.0 times to ensure the reduction amount of the finishing pass.

6. The method for producing structural steel for construction machinery according to claim 5, characterized in that: In the rolling process, the final rolling temperature is controlled below 820°C.

7. The method for producing structural steel for construction machinery according to claim 5, characterized in that: The steel plates are air-cooled after rolling.