Low-temperature-resistant high-toughness flat-bulb steel and preparation method thereof

By adding Fe2(MoO4)3 powder to the ball flat steel, the raw material ratio is optimized, and the problems of high production cost and insufficient toughness of ball flat steel are solved, and excellent performance and economic benefits are improved at low temperatures, which is in line with GB/T 9945 -2012 standard.

CN118979194AInactive Publication Date: 2024-11-19CHANGSHU LONGTENG SPECIAL STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411059756.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing ball flat steel has high production costs and insufficient toughness, especially due to the poor economic benefits caused by the use of precious metals Nb and Cr, and the toughness needs to be improved.

Method used

By preparing Fe2(MoO4)3 powder and adding it to the ball flat steel, the raw material ratio is optimized, including C, Mn, scrap steel, S, Si, Ba and Fe, and a yellow precipitate is used to react with ferrous nitrate and sodium peroxide solution to form a yellow precipitate. Reacted with ammonium heptamolybdate solution to produce Fe2(MoO4)3 powder, which is used for smelting and rolling to prepare low-temperature and high-toughness ball flat steel.

Benefits of technology

The obtained ball flat steel has excellent performance, high toughness and improved elongation at low temperatures. It also avoids the use of precious metals, reduces production costs and improves economic benefits, and complies with the GB/T 9945-2012 standard.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a low-temperature-resistant high-toughness flat-bulb steel, which belongs to the technical field of flat-bulb steel, and comprises the following raw materials by weight: 0.07-0.09% of C; mn: 0.46 to 0.83%; 0.06 to 0.08% of waste steel; 0.14% to 0.18% of S; 0.07% to 0.12% of Si; 0.02 to 0.05 percent of Ba; 0.025%-0.041% of Fe2 (MoO4) 3: (0. And the balance of Fe. The preparation method of the Fe2 (MoO4) 3 comprises the following steps: A, dropwise adding a sodium peroxide solution into a ferrous nitrate solution until the solution turns yellow to generate a solution A containing ferric nitrate; b, heating the solution A, and keeping the temperature for a period of time; dropwise adding a preheated ammonium heptamolybdate solution while stirring to generate a yellow precipitate; and C, centrifuging to obtain a precipitate, and drying the precipitate to obtain Fe2 (MoO4) 3 powder. By optimizing the proportion of all the components, the prepared flat-bulb steel is excellent in performance and high in toughness at the low temperature, the ductility is effectively improved by adding Fe2 (MoO4) 3, in addition, the used raw materials are low in price, use of precious metal is avoided, and therefore the production cost is effectively reduced, and economic benefits are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bulb flat steel, and in particular to a bulb flat steel material with low temperature resistance and high toughness and a preparation method thereof. Background Art

[0002] Bulb flat steel is a kind of special steel, mainly used in shipbuilding and bridge building. However, with the rapid development of the shipbuilding industry in recent years, bulb flat steel has gradually become a special name for marine bulb flat steel. It is the most important type of marine steel, mainly used as reinforcement of ship plates, which is equivalent to human "ribs".

[0003] For example, Chinese patent CN117305716B proposes a method for preparing a seismic and corrosion-resistant bulb flat steel, which belongs to the field of structural steel technology. The method for preparing the seismic and corrosion-resistant bulb flat steel is: a complex phase structure consisting of ferrite + bainite + residual austenite with good comprehensive performance is obtained through controlled rolling and controlled cooling and online overaging treatment, and the strength is improved by refining the grains through Nb and N microalloying, and the corrosion resistance is improved by adding Cu and Cr.

[0004] However, the Nb and Cr used in the above patents are relatively expensive, which increases the production cost and the economic benefits need to be improved; and the toughness needs to be further improved.

[0005] Based on this, the present invention designs a low-temperature resistant and high-toughness bulb flat steel and a preparation method thereof to solve the above problems. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a low-temperature resistant and high-toughness bulb flat steel and a preparation method thereof.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A low temperature resistant and high toughness bulb flat steel material comprises the following raw materials in weight percentage: C: 0.07-0.09%; Mn: 0.46-0.83%; scrap steel: 0.06-0.08%; S: 0.14-0.18%; Si: 0.07-0.12%; Ba: 0.02-0.05%; Fe2(MoO4)3: 0.025-0.041%; the balance is Fe;

[0009] The preparation method of the Fe2(MoO4)3 is as follows:

[0010] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0011] B. Heat solution A and keep it warm for a period of time; add the preheated ammonium heptamolybdate solution dropwise while stirring to generate a yellow precipitate;

[0012] C. Centrifuge and take out the precipitate, then dry the precipitate to obtain Fe2(MoO4)3 powder.

[0013] A method for preparing a low-temperature resistant and high-toughness bulb flat steel comprises the following steps:

[0014] Step 1: Preparation of Fe2(MoO4)3;

[0015] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0016] B. Heat solution A and keep it warm; add the preheated ammonium heptamolybdate solution dropwise while stirring to generate a yellow precipitate;

[0017] C. Centrifuge and take the precipitate, and dry the precipitate to obtain Fe2(MoO4)3 powder;

[0018] Step 2: Smelt the raw materials into molten iron and slowly add Fe2(MoO4)3 powder;

[0019] Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0020] Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

[0021] Furthermore, in step A, the molar ratio of ferrous nitrate to sodium peroxide is 1:1.2-1.5.

[0022] Furthermore, step B is specifically as follows: heating solution A to 60-70° C. and keeping the temperature for 30-40 minutes; adding dropwise an ammonium heptamolybdate solution preheated to 80° C. while stirring to generate a yellow precipitate.

[0023] Furthermore, in step B, the mass ratio of solution A to ammonium heptamolybdate solution is 14:3-5.

[0024] Furthermore, the Fe2(MoO4)3 powder has a particle size of 50-70 μm.

[0025] Furthermore, in step B, the dropping speed is 10 drops / min.

[0026] Furthermore, step 2 is specifically as follows: smelting the raw materials into molten iron at 1180-1230°C, slowly adding Fe2(MoO4)3 powder, and completing the addition within 20 minutes.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The bulb flat steel produced by the present invention complies with the GB / T 9945-2012 standard; by optimizing the ratio of each component, the bulb flat steel has excellent performance at low temperature and high toughness, and the elongation is effectively improved by adding Fe2(MoO4)3. In addition, the raw materials used in the present invention are relatively low in price, and the use of precious metals is avoided, thereby effectively reducing production costs and improving economic benefits. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1

[0031] This embodiment provides a low temperature resistant and high toughness bulb flat steel material, comprising the following steps:

[0032] Step 1: Preparation of Fe2(MoO4)3;

[0033] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0034] The molar ratio of ferrous nitrate to sodium peroxide is 1:1.5;

[0035] B. Heat solution A to 70°C and keep it warm for 30-40 minutes; add the ammonium heptamolybdate solution preheated to 80°C dropwise while stirring to generate a yellow precipitate; the dropping speed is 10 drops / min;

[0036] The mass ratio of solution A to ammonium heptamolybdate solution is 14:3-5;

[0037] C. Centrifuge and take the precipitate, and dry the precipitate to obtain Fe2(MoO4)3 powder with a particle size of 50-70 μm;

[0038] Step 2: weigh the raw materials: C powder: 0.09%; Mn powder: 0.83%; scrap steel powder: 0.08%; S powder: 0.18%; Si powder: 0.12%; Ba powder: 0.05%; Fe2(MoO4)3 powder: 0.041%; the rest is Fe powder;

[0039] The raw materials were melted into molten iron at 1230℃, and Fe2(MoO4)3 powder was slowly added in 20 minutes;

[0040] Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0041] Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

[0042] Embodiment 2

[0043] This embodiment provides a low temperature resistant and high toughness bulb flat steel material, comprising the following steps:

[0044] Step 1: Preparation of Fe2(MoO4)3;

[0045] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0046] The molar ratio of ferrous nitrate to sodium peroxide is 1:1.2;

[0047] B. Heat solution A to 60°C and keep it warm for 30 minutes; add the ammonium heptamolybdate solution preheated to 80°C dropwise while stirring to generate a yellow precipitate; the dropping speed is 10 drops / min;

[0048] The mass ratio of solution A to ammonium heptamolybdate solution is 14:3;

[0049] C. Centrifuge and take out the precipitate, and dry the precipitate to obtain Fe2(MoO4)3 powder with a particle size of 50 μm;

[0050] Step 2: weigh the raw materials: C powder: 0.07%; Mn powder: 0.46%; scrap steel powder: 0.06%; S powder: 0.14%; Si powder: 0.07%; Ba powder: 0.02%; Fe2(MoO4)3 powder: 0.025%; the rest is Fe powder;

[0051] The raw materials were melted into molten iron at 1180℃, and Fe2(MoO4)3 powder was slowly added in 20 minutes;

[0052] Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0053] Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

[0054] Embodiment 3

[0055] This embodiment provides a low temperature resistant and high toughness bulb flat steel material, comprising the following steps:

[0056] Step 1: Preparation of Fe2(MoO4)3;

[0057] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0058] The molar ratio of ferrous nitrate to sodium peroxide is 1:1.4;

[0059] B. Heat solution A to 68°C and keep it warm for 34 minutes; add the ammonium heptamolybdate solution preheated to 80°C dropwise while stirring to generate a yellow precipitate; the dropping speed is 10 drops / min;

[0060] The mass ratio of solution A to ammonium heptamolybdate solution is 14:4;

[0061] C. Centrifuge and take the precipitate, and dry the precipitate to obtain Fe2(MoO4)3 powder with a particle size of 50-70 μm;

[0062] Step 2: weigh the raw materials: C powder: 0.08%; Mn powder: 0.61%; scrap steel powder: 0.07%; S powder: 0.16%; Si powder: 0.09%; Ba powder: 0.04%; Fe2(MoO4)3 powder: 0.032%; the rest is Fe powder;

[0063] The raw materials were melted into molten iron at 1210℃, and Fe2(MoO4)3 powder was slowly added in 20 minutes;

[0064] Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0065] Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

[0066] Comparative Example 1

[0067] Different from Example 3, no Fe2(MoO4)3 powder was added;

[0068] This embodiment provides a low temperature resistant and high toughness bulb flat steel material, comprising the following steps:

[0069] Step 1: weigh the raw materials: C powder: 0.08%; Mn powder: 0.61%; scrap steel powder: 0.07%; S powder: 0.16%; Si powder: 0.09%; Ba powder: 0.04%; the rest is Fe powder;

[0070] The raw materials are melted into molten iron at 1210°C;

[0071] Step 2: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0072] Step 3: Cooling, splitting and straightening to obtain bulb-flat steel.

[0073] Comparative Example 2

[0074] Different from Example 3, in step B, solution A and ammonium heptamolybdate solution were not preheated;

[0075] This embodiment provides a low temperature resistant and high toughness bulb flat steel material, comprising the following steps:

[0076] Step 1: Preparation of Fe2(MoO4)3;

[0077] A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate;

[0078] The molar ratio of ferrous nitrate to sodium peroxide is 1:1.4;

[0079] B. Add ammonium heptamolybdate solution to solution A dropwise while stirring to generate a yellow precipitate; the dropping speed is 10 drops / min;

[0080] The mass ratio of solution A to ammonium heptamolybdate solution is 14:4;

[0081] C. Centrifuge and take the precipitate, and dry the precipitate to obtain Fe2(MoO4)3 powder with a particle size of 50-70 μm;

[0082] Step 2: weigh the raw materials: C powder: 0.08%; Mn powder: 0.61%; scrap steel powder: 0.07%; S powder: 0.16%; Si powder: 0.09%; Ba powder: 0.04%; Fe2(MoO4)3 powder: 0.032%; the rest is Fe powder;

[0083] The raw materials were melted into molten iron at 1210℃, and Fe2(MoO4)3 powder was slowly added in 20 minutes;

[0084] Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle;

[0085] Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

[0086] Experimental example

[0087] The bulb flat steel produced by the present invention complies with the GB / T 9945-2012 standard;

[0088] The bulb flat steels prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to a -60°C Charpy V-notch pendulum impact test according to the standard of GB / T 19748-2019;

[0089] The ductility was tested according to GB / T 15821-1995 standard, and the results are as follows:

[0090] project Embodiment 1 Embodiment 2 Embodiment 3 Comparative Example 1 Comparative Example 2 Impact energy J 191 185 187 125 148 Elongation % 18 17 19 15 17

[0091] As can be seen from the above table, the present invention optimizes the ratio of each component so that the obtained bulb flat steel has excellent performance and high toughness at low temperature, and the elongation is effectively improved by adding Fe2(MoO4)3.

[0092] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low temperature resistant and high toughness bulb flat steel. Features: The invention comprises the following raw materials in weight percentage: C: 0.07-0.09%; Mn: 0.46-0.83%; Scrap steel: 0.06-0.08%; S: 0.14-0.18%; Si: 0.07-0.12%; Ba: 0.02-0.05%; Fe: 2 (MoO 4 ) 3 : 0.025-0.041%; Remaining amount Fe; The Fe 2 (MoO 4 ) 3 The preparation method is as follows: A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate; B. Heat solution A and keep it warm for a period of time; Add the preheated ammonium heptamolybdate solution dropwise while stirring to generate a yellow precipitate; C. Centrifuge and take the precipitate, dry the precipitate to obtain Fe 2 (MoO 4 ) 3 powder.

2. A method for preparing a low temperature resistant and high toughness bulb flat steel. It is characterized in that The following steps are involved: Step 1: Preparation of Fe 2 (MoO 4 ) 3 ; A. Add sodium peroxide solution dropwise to the ferrous nitrate solution until the solution turns yellow to generate solution A containing ferric nitrate; B. Heat solution A and keep it warm; add the preheated ammonium heptamolybdate solution dropwise while stirring to generate a yellow precipitate; C. Centrifuge and take the precipitate, dry the precipitate to obtain Fe 2 (MoO 4 ) 3 powder; Step 2: Smelt the raw materials into molten iron and slowly add Fe 2 (MoO 4 ) 3 powder; Step 3: Continuously casting and rolling to obtain thick ends at both ends and a thin plate in the middle; Step 4: Cooling, splitting and straightening to obtain bulb-flat steel.

3. The preparation method according to claim 2, It is characterized in that In step A, the molar ratio of ferrous nitrate to sodium peroxide is 1:1.2-1.

5.

4. The preparation method according to claim 3, It is characterized in that Step B is specifically as follows: heating solution A to 60-70° C. and keeping the temperature for 30-40 minutes; adding dropwise an ammonium heptamolybdate solution preheated to 80° C. while stirring to generate a yellow precipitate.

5. The preparation method according to claim 4, It is characterized in that In step B, the mass ratio of solution A to ammonium heptamolybdate solution is 14:3-5.

6. The preparation method according to claim 5, It is characterized in that The Fe 2 (MoO 4 ) 3 Powder particle size 50-70μm.

7. The preparation method according to claim 6, It is characterized in that In step B, the dropping speed is 10 drops / min.

8. The preparation method according to claim 7, It is characterized in that Step 2 is as follows: smelt the raw materials into molten iron at 1180-1230℃, slowly add Fe 2 (MoO 4 ) 3 Powder, add in 20 minutes.

Citation Information

Patent Citations

  • Graphene clad Fe2(MoO4)3 nanoparticle and preparation method and application thereof

    CN105742598A

  • Method for making ferromolybdenum alloy powder

    CN1065419A

  • Q345FRQ fire-resisting and earthquake-proof hot rolling angle steel used for public steel structure buildings and preparing method of Q345FRQ fire-resisting and earthquake-proof hot rolling angle steel

    CN106906411A

  • Shape steel material having high strength, high toughness and excellent fire resistance and process for producing rolled shape steel of said material

    CN1088628A

  • Amorphous Fe-Mo-O coated Fe2(MoO4)3 lithium ion battery negative electrode material and preparation method thereof

    CN110416505A