Method for improving toughness of ZL205A alloy
Through homogenization treatment and hot extrusion technology, combined with the microalloyation and heat treatment of the rare earth element Sc, the problem of ZL205A aluminum alloy is solved between high strength and high toughness, significantly improving its strength and plasticity, and improving casting Performance, suitable for a variety of high-end applications.
Patent Information
- Application Number
- CN202411085828.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
ZL205A aluminum alloy is difficult to take into account between high strength and high toughness, and has poor casting performance, which has thermal cracking, casting defects and segregation problems, affecting its strength and toughness.
Through homogenization treatment and hot extrusion technology, dendrite segregation and eutectic phases in the structure are eliminated to form fine and uniform second phase particles, and the microalloyation and heat treatment of the rare earth element Sc are combined to improve the mechanical properties of the alloy.
It significantly improves the strength and plasticity of ZL205A alloy, improves casting performance, is suitable for a variety of high-end applications, expands its application range and enhances market competitiveness.
Smart Images

Figure CN118979208A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy preparation, and in particular relates to a method for improving the strength and toughness of a ZL205A alloy. Background Art
[0002] With the development of the automotive industry, engineering machinery, and civil equipment, people have higher and higher requirements for aluminum alloy materials. At the same time, higher strength aluminum alloy materials have received more and more attention from all walks of life. The problem that still exists in the current application of high-strength cast aluminum alloys is that high-strength cast aluminum alloy materials often cannot meet the requirements of high strength and high toughness while meeting the requirements of lightweight, and improve their service stability in complex environments.
[0003] ZL205A alloy is the second generation of cast aluminum alloy of A1-Cu series. Due to the solid solution strengthening and precipitation strengthening of numerous trace elements, the alloy has extremely high room temperature and high temperature mechanical properties. It is one of the strongest cast aluminum alloys and is widely used in the fields of transportation manufacturing and high-performance structural parts manufacturing. ZL205A alloy has good welding performance and machining performance, but poor casting performance, poor corrosion resistance, and a large linear expansion coefficient. In the casting production process, there are mainly problems such as hot cracking, casting defects (such as shrinkage, shrinkage, impurities) and casting segregation. These problems will have a great impact on the quality and toughness of the final casting, resulting in its toughness not meeting the standards in some application scenarios. How to avoid or reduce these problems in the casting production process is the only way to improve the toughness of ZL205A alloy.
[0004] In summary, the ZL205A alloy also places higher requirements on its high strength and toughness in the context of wide application in engineering. How to effectively improve the strength and toughness of the ZL205A alloy through simple means requires more in-depth research. Summary of the invention
[0005] In view of the above-mentioned prior art, the purpose of the present invention is to provide a method for improving the strength and toughness of ZL205A alloy, so as to solve the problem that the strength and toughness of the existing ZL205A alloy are insufficient.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a method for improving the strength and toughness of ZL205A alloy is provided, comprising the following steps:
[0007] S1: homogenizing the ZL205A alloy and then cooling it;
[0008] S2: ZL205A alloy and extrusion die after preheating and homogenization treatment;
[0009] S3: Put the preheated ZL205A alloy into the preheated extrusion die, and then transfer it to the extruder for extrusion. The extrusion speed is 2-6 mm / s, the extrusion temperature is 300-500°C, and the extrusion ratio is ≥4.
[0010] The beneficial effects of the present invention are as follows: a large number of network-shaped and block-shaped coarse θ(Al2Cu) phases exist in the ZL205A cast alloy. After homogenization treatment, the θ(Al2Cu) phases can be dissolved into the matrix and the serious dendrite segregation in the organization can be eliminated, so that the residual eutectic phase and the insoluble particles are reduced, the alloy element segregation is also improved, and the distribution is more uniform.
[0011] After hot extrusion of the homogenized alloy, the void defects are eliminated, and a large number of uniform, fine and dispersed second phase particles appear inside the extruded alloy. These particles have a pinning effect on grain boundaries and dislocations during deformation, and the broken second phase particles can hinder the growth of recrystallized grains, thereby playing a role in grain refinement, which is beneficial to microstructure refinement and improving the mechanical properties of the alloy.
[0012] On the basis of the above technical solution, the present invention can also be improved as follows:
[0013] Furthermore, the homogenization treatment was carried out at 500° C. for 12 h.
[0014] Further, the preheating temperature of the ZL205A alloy is 30°C higher than the preheating temperature of the extrusion die, and the preheating time is 30min.
[0015] Furthermore, the extrusion speed was 4 mm / s and the extrusion temperature was 350°C.
[0016] Furthermore, it also includes:
[0017] S4: The ZL205A alloy treated by S3 is subjected to solution treatment and aging treatment in sequence, and then air-cooled to room temperature.
[0018] Furthermore, the solution treatment is carried out at 500-540°C for 14 hours, and the aging treatment is carried out at 175°C for 4 hours.
[0019] Furthermore, rare earth elements are added to the ZL205A alloy before homogenization treatment.
[0020] Furthermore, the rare earth element is Sc.
[0021] Furthermore, the addition amount of Sc is 0.05 to 0.2 wt % of the ZL205A alloy.
[0022] Further, the operation steps of adding rare earth elements are:
[0023] S1: Add ZL205A alloy and rare earth elements into a resistance furnace for melting and heat to 740℃;
[0024] S2: Degassing with argon, then continue heating to 760°C, refining and keeping the temperature for 20 minutes;
[0025] S3: Pour the melt into a metal mold and cool it.
[0026] The present invention has the following beneficial effects:
[0027] 1. The present invention improves the strength and toughness of ZL205A alloy by means of casting process optimization, Sc microalloying, hot extrusion and heat treatment. During the extrusion process, the alloy forms a dense structure, refines the grains, and forms a large number of uniformly finely dispersed high-temperature resistant second phase particles that have a pinning effect on grain boundaries and dislocations. These particles can prevent grain growth in the subsequent solution treatment, so that the material ultimately obtains high strength and plasticity, that is, high strength and toughness; the addition of Sc elements generates Sc-containing second phases as heterogeneous nucleation cores in the billet casting stage, and refines the cast grains. At the same time, through hot extrusion and subsequent heat treatment, a large number of fine and dispersed Sc-containing second phases can be formed in the matrix, which have a strong pinning effect on the grain boundaries, and finally obtain finer matrix grains, so the strength and plasticity of the alloy are further improved.
[0028] 2. The process of the present invention is simple and can meet different requirements for high plasticity or high strength of ZL205A aluminum alloy under different environments, and is suitable for promotion and application.
[0029] 3. Traditional cast aluminum alloys are difficult to use for plastic processing due to their low plasticity. The present invention significantly improves the plasticity of ZL205A alloy through hot extrusion and heat treatment, so that it can also be plastic processed into parts of various shapes and sizes, greatly expanding the application scope of the aluminum alloy, with application prospects in multiple high-end fields, and improving its comprehensive performance and market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The metallographic microstructures of the alloys prepared in Comparative Example 1 and Comparative Example 2 are shown in Figure (a) for Comparative Example 1 and Figure (b) for Comparative Example 2;
[0031] Figure 2 The microstructure diagrams of the cross sections of the alloys prepared in Examples 1-2 and Comparative Example 3 are shown in Figure (a) for Example 2, Figure (b) for Example 1, and Figure (c) for Comparative Example 3;
[0032] Figure 3The SEM microstructure images of the longitudinal sections of the alloys prepared in Examples 1-2 and Comparative Example 3, wherein (a) is Example 2, (b) is Example 1, and (c) is Comparative Example 3;
[0033] Figure 4 The SEM microstructure diagrams of the longitudinal sections of the alloys prepared in Example 1, Example 3 and Example 4, wherein Figure (a) is Example 3, Figure (b) is Example 1, and Figure (c) is Example 4;
[0034] Figure 5 EBSD analysis results of the longitudinal sections of the alloys prepared in Example 1 and Example 5, wherein Figure (a) is Example 1, and Figure (b) is Example 5;
[0035] Figure 6 EBSD analysis results of the longitudinal sections of the alloys prepared in Example 7 and Example 8, wherein Figure (a) is Example 7, and Figure (b) is Example 8;
[0036] Figure 7 The SEM microstructure images of the alloy prepared in Example 8, wherein Figure (ab) is a cross section and Figure (cd) is a longitudinal section. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0038] Example 1
[0039] A hot extrusion process of a ZL205A alloy comprises the following steps:
[0040] (1) Homogenization
[0041] The ZL205A ingot was placed in an integrated muffle furnace (SX2-4-10A, temperature error <±5°C) for homogenization treatment at a homogenization temperature of 500°C for 12 h, and then air-cooled to room temperature (natural cooling in air).
[0042] (2) Hot extrusion
[0043] S21: The homogenized ZL205A ingot is processed into a 30 mm × 40 mm round ingot, and the round ingot and the die are preheated for 30 min using an integrated muffle furnace and a ring electric furnace (CH400 × 100, temperature error < ± 5 ° C), wherein the preheating temperature of the round ingot is 350 ° C, and the preheating temperature of the die is 320 ° C; the die material is D2 die steel, the outer diameter of the die is 35 mm, and the inner diameter of the die is 10 mm;
[0044] S22: The preheated ingot is placed into the preheated extrusion die, and then transferred to a vertical forward extruder (YH-200t) for extrusion at an extrusion speed of 4 mm / s, an extrusion temperature of 350°C, an extrusion ratio of 9:1, and a forward extrusion pressure of 200t to obtain an extruded rod.
[0045] Example 2
[0046] The extrusion temperature of S22 in Example 1 is replaced with 300° C., and the remaining steps are the same as in Example 1.
[0047] Example 3
[0048] The extrusion speed of S22 in Example 1 is replaced with 2 mm / s, and the remaining steps are the same as in Example 1.
[0049] Example 4
[0050] The extrusion speed of S22 in Example 1 is replaced with 6 mm / s, and the remaining steps are the same as in Example 1.
[0051] Example 5
[0052] A hot extrusion + heat treatment process of ZL205A alloy, comprising the following steps:
[0053] The extruded rod prepared in Example 1 was added to a box-type resistance furnace (SX-8-10, temperature error <±5°C) for solution treatment and aging treatment in sequence. The solution treatment parameters were 538°C×14h, and the aging treatment parameters were 175°C×4h, and then air-cooled to room temperature.
[0054] Example 6
[0055] The aging treatment parameters in Example 5 were replaced with 190° C.×3 h, and the remaining steps were the same as in Example 5.
[0056] Example 7
[0057] The aging treatment parameters in Example 5 were replaced with 155° C.×9 h, and the remaining steps were the same as in Example 5.
[0058] Example 8
[0059] A process of Sc microalloying+hot extrusion+heat treatment of ZL205A alloy, comprising the following steps:
[0060] (1) Sc microalloying
[0061] S11: a layer of coating is applied to the cavity of the metal casting mold and dried at high temperature, the ZL205A ingot is added to an industrial resistance furnace (J2-75-9, temperature error <±5°C), heated to melt, and then Al-2Sc is added to make the Sc content 0.1wt% of the alloy, stirred evenly, and then heated to 740°C;
[0062] S12: Degassing with argon (purity not less than 99.98%) for 8 minutes, when the temperature increases to 760°C, refining is performed and heat preservation is performed for 20 minutes;
[0063] S13: After the heat preservation is completed, the melt is poured from the crucible into a 90 mm Φ cylindrical metal mold cavity preheated to 200° C. at a speed of 0.12 kg / s, and cooled to obtain a casting.
[0064] (2) Homogenization
[0065] The casting was placed in an integrated muffle furnace (SX2-4-10A, temperature error <±5°C) for homogenization treatment at a homogenization temperature of 500°C for 12 h, and then air-cooled to room temperature (natural cooling in air).
[0066] (3) Hot extrusion
[0067] S31: The ZL205A ingot after homogenization treatment is processed into a 30mm×40mm round ingot, and the round ingot and the die are preheated for 30 minutes using an integrated muffle furnace and a ring electric furnace (CH400×100, temperature error <±5°C), wherein the preheating temperature of the round ingot is 350°C, and the preheating temperature of the die is 320°C; the die material is D2 die steel, the outer diameter of the die is 35mm, and the inner diameter of the die is 10mm;
[0068] S32: The preheated ingot is placed into the preheated extrusion die, and then transferred to a vertical forward extruder (YH-200t) for extrusion at an extrusion speed of 4 mm / s, an extrusion temperature of 350°C, an extrusion ratio of 9:1, and a forward extrusion pressure of 200t to obtain an extruded rod.
[0069] (4) Heat treatment
[0070] The extruded bars were added into a box-type resistance furnace (SX-8-10, temperature error <±5°C) for solution treatment and aging treatment in sequence. The solution treatment parameters were 538°C×14h, and the aging treatment parameters were 175°C×4h, and then air-cooled to room temperature.
[0071] Comparative Example 1
[0072] Untreated ZL205A ingot.
[0073] Comparative Example 2
[0074] A homogenization process for ZL205A alloy comprises the following steps:
[0075] The ZL205A ingot was placed in an integrated muffle furnace (SX2-4-10A, temperature error <±5°C) for homogenization treatment at a homogenization temperature of 500°C for 12 h, and then air-cooled to room temperature (natural cooling in air).
[0076] Comparative Example 3
[0077] The extrusion temperature of S22 in Example 1 is replaced with 500° C., and the remaining steps are the same as in Example 1.
[0078] Experimental Example 1: Alloy Mechanical Properties Test
[0079] The yield strength, tensile strength and elongation of the alloys prepared in Examples 1-8 and Comparative Examples 1-3 were tested. The test results are shown in Table 2.
[0080] Table 2 Mechanical properties of alloys at room temperature
[0081]
[0082] Based on the above data, it can be concluded that compared with comparative examples 1-3, the strength and toughness of the alloys prepared in examples 1-8 are greatly improved.
[0083] From the data of Examples 1-2 and Comparative Example 3, it can be seen that the yield strength and tensile strength of the extruded ZL205A alloy show a trend of first increasing and then decreasing with the increase of the extrusion temperature. When the extrusion temperature is low, the fluidity of the alloy is low and the resistance during extrusion is large. When the extrusion temperature is high, the plasticity of the alloy decreases slightly. Taking all factors into consideration, the optimal extrusion temperature is 350°C.
[0084] From the data of Example 1, Example 3 and Example 4, it can be seen that the yield strength, elongation and static toughness at an extrusion speed of 4 mm / s are better than those at other extrusion rates, among which the yield strength and static toughness have obvious advantages, and the elongation fluctuates little; the strengthening effect on the mechanical properties of the alloy bar during the extrusion process mainly comes from grain refinement. Since the extrusion temperature is the same and the extrusion speed is different during the extrusion process, the instantaneous temperature and cooling rate during the extrusion process are different but the total time is very short, so the mechanical properties at different extrusion rates are close.
[0085] In Examples 5-7, the ZL205A extruded samples after solution treatment at 538°C for 14 hours were subjected to different aging treatments, namely, aging at 155°C for 9 hours, aging at 175°C for 4 hours, and aging at 190°C for 3 hours. From the data in the table, it can be seen that the yield strength and tensile strength of the alloys of Examples 6-8 are greatly improved, and the plasticity is slightly decreased. This is because a strengthening phase will precipitate after the aging treatment, which will have a positive effect on the strength of the alloy. Although the hardness of the strengthening phase is high, the strengthening phase is not easy to deform, which has an adverse effect on the plasticity of the alloy. Among the three aging treatments, aging at 175°C for 4 hours is the optimal aging treatment system.
[0086] Example 8: A ZL205A alloy with a Sc content of 0.1% is hot extruded at a temperature of 350°C, a speed of 4 mm / s, and an extrusion ratio of 9:1, and is subjected to T6 heat treatment. The three processes are combined to synergistically improve the strength and toughness of the ZL205A alloy, and its yield strength and tensile strength are significantly improved, meeting the expected service performance requirements.
[0087] During casting, the appropriate combination process can be selected according to the different requirements for high plasticity or high strength of ZL205A aluminum alloy in different environments.
[0088] Experimental Example 2: Alloy Metallographic Structure Analysis
[0089] Optical metallographic structure observation (OM), scanning electron microscope observation (SEM) and electron backscatter diffraction analysis (EBSD) were performed on the alloys prepared in Examples 1-8 and Comparative Examples 1-3.
[0090] Figure 1 The metallographic microstructure diagrams of the alloys prepared in Comparative Example 1 and Comparative Example 2 (a-Comparative Example 1, b-Comparative Example 2) show that a large number of coarse second phases in the form of mesh and block exist at the grain boundaries of the cast alloy in the untreated ZL205A ingot in Comparative Example 1, which are determined to be θ(Al2Cu) phases by EDS analysis. They are interconnected to separate the grains and aggregate at the grain boundaries; the distribution of Cu element in the matrix is uneven, mainly aggregated and distributed at the grain boundaries, forming a θ(Al2Cu) phase with a clear mesh structure; except for V and Zr, which aggregate in small amounts at the grain boundaries to form a high temperature resistant phase, the distribution of other elements is relatively uniform. After homogenization treatment, most of the θ(Al2Cu) phases have been dissolved into the matrix, the mesh θ(Al2Cu) phases are eliminated, the grain boundaries are continuous and smooth, the residual eutectic phases and insoluble particles at the grain boundaries are less, and the alloy structure is improved.
[0091] Figure 2The cross-sectional microstructure diagrams of the alloys prepared in Examples 1-2 and Comparative Example 3 at different extrusion temperatures (a-300℃, b-350℃, c-500℃) are shown. The degree of recrystallization of the extruded rod can be distinguished by using a corrosive agent to corrode the subgrain boundaries with large orientation differences. From the cross-sectional corrosion results perpendicular to the extrusion direction, it can be seen that the white bright spot area is the recrystallization area, and the non-recrystallized grains appear black due to the large number of small subgrains inside. The recrystallized area gradually increases with the increase of the extrusion temperature, and the non-recrystallized area gradually decreases; after extrusion, the grains in the longitudinal section are elongated along the extrusion direction and arranged in a fibrous manner, the grain boundary contours become blurred, and the grains tend to grow with the increase of the extrusion temperature.
[0092] Figure 3 The SEM microstructures of the longitudinal sections of the alloys prepared in Examples 1-2 and Comparative Example 3 at different hot extrusion temperatures (a-300°C, b-350°C, e-500°C) show that the mesh and irregular second phases in the cast state after the hot extrusion process are broken into micron-sized particles distributed at the grain boundaries during the hot extrusion deformation process, and are arranged in strips along the extrusion direction. At 350°C, more broken second phases are shown in the SEM image, and the broken second phase particles at 500°C are the least, because part of the heat generated during the hot extrusion process causes the temperature to rise. As the extrusion temperature increases, the temperature inside the alloy gradually increases from close to the dynamic recrystallization temperature to above the recrystallization temperature. Excessively high temperatures will dissolve some of the fine second phases, resulting in a decrease in quantity, so the number of precipitated phases shows a trend of first increasing and then decreasing.
[0093] Figure 4 The SEM microstructure diagrams (a-2mm / s, b-4mm / s, c-6mm / s) of the longitudinal sections of the alloys prepared in Example 1, Example 3 and Example 4 at different extrusion speeds show that the second phase particles crushed by extrusion on the longitudinal sections of the alloys are distributed in a band along the extrusion direction at different extrusion speeds. When the extrusion speed is low, the longitudinal section of the extruded rod has fewer crushed second phase particles and a small amount of recrystallized grains are generated inside. When the extrusion temperature remains unchanged, when the extrusion speed of the alloy increases, more recrystallized grains will gradually be generated inside the alloy. The extrusion speed of the alloy has a significant effect on the amount of heat generated by the deformed material and the length of the heat exchange time provided. To a certain extent, as the extrusion speed increases, more recrystallized grains are gradually generated inside the alloy, but too high an extrusion speed will cause the size and distribution of the second phase particles to change. When the extrusion rate is 4mm / s, there are more crushed second phases inside the alloy, and the dispersibility and uniformity are relatively better. At this time, the extruded rod has the best mechanical properties.
[0094] In Examples 5 to 7 of the present invention, different aging treatments were performed on the alloy (T5 / 155°C×9h / Example 7, T6 / 175°C×4h / Example 5, T7 / 190°C×3h / Example 6). It can be found through observation that the distribution and size of the undissolved high-temperature phases did not change much under the three aging systems, and the performance changes were mainly caused by the differences in the nanoscale precipitated phases. Comprehensive consideration showed that the best aging treatment system was the T6 aging treatment.
[0095] Figure 5 The EBSD analysis results of the longitudinal section of the alloy extruded material under the T6 aging system (a-before T6 heat treatment / Example 1, b-after T6 heat treatment / Example 5). From Figure (a), it can be found that after hot extrusion treatment, the equiaxed grains in the homogeneous alloy deform under the influence of extrusion stress, causing the grains to deform along the extrusion direction, from equiaxed crystals to thin and long fibrous grains with layered distribution. The three colors of red, green and blue are used in the figure to represent <001> , <101> , <111> Oriented grains, grains of the same color have the same orientation. Through observation, it can be found that the fine equiaxed grains produced after extrusion are mainly red. After T6 heat treatment, it can be found that the grain orientation distribution has hardly changed, among which the red fine grains have grown significantly. This is because the broken second phase produced during the extrusion process and the fine equiaxed crystals formed by recrystallization grow along the extrusion direction into fibrous long grains.
[0096] Figure 6 The EBSD analysis results of the longitudinal sections of the alloys of Example 7 (no Sc added, Figure a) and Example 8 (0.1% Sc added, Figure b) show that after adding the Sc element, the alloy grains become significantly finer and are distributed in a fibrous manner along the extrusion direction. This is because the addition of the Sc element greatly inhibits the occurrence of recrystallization and prevents the growth of recrystallized grains, thereby making the grains finer.
[0097] Figure 7 The SEM microstructure diagram of the alloy with 0.1% Sc added in Example 8 (a / b- cross section, c / d- longitudinal section). Through observation, it can be found that there are many second phase particles with different size distributions in the cross section, which are generally uniform and fine particles, with only a small number of large-sized particles, distributed in islands and strips. After EDS analysis, the particles with strip distribution are mainly the θ(Al2Cu) phase broken during the extrusion process.
[0098] In summary, after hot extrusion treatment, the equiaxed grains in the homogeneous alloy deform along the extrusion direction under the action of extrusion stress, and the original equiaxed grains are transformed into slender fibrous grains. This shows that during the hot extrusion deformation process, a large number of dislocations accumulate and entangle in the grains, forming small-angle grain boundaries and a small number of high-angle grain boundaries. In addition, dislocations will accumulate at the original grain boundaries, promoting the formation of a large number of substructures with various orientations at the grain boundaries, so that new fine grains appear at the grain boundaries of the original grains, distributed along the extrusion direction. The addition of Sc element can inhibit the occurrence of recrystallization. The recrystallization texture in the extruded rod with 0.1% Sc added is <101> The strength is reduced, and the corresponding non-recrystallized deformation texture caused by hot extrusion is significantly enhanced. The addition of Sc element to improve the strength and toughness of the alloy is mainly attributed to the increase of nucleation cores during the solidification of AlSc phase, and its undissolved particles hinder the movement of grain boundaries during the solution process, eventually forming fine grains. At the same time, the nano-sized AlSc precipitated during the aging heat treatment has a strong pinning effect on dislocations and subgrain boundaries, further improving the strength of the material.
[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for improving the strength and toughness of ZL205A alloy, characterized in that: The following steps are involved: S1: homogenizing the ZL205A alloy and then cooling it; S2: ZL205A alloy and extrusion die after preheating and homogenization treatment; S3: Put the preheated ZL205A alloy into the preheated extrusion die, and then transfer it to the extruder for extrusion. The extrusion speed is 2-6 mm / s, the extrusion temperature is 300-450°C, and the extrusion ratio is ≥4.
2. The method for improving the strength and toughness of ZL205A alloy according to claim 1, characterized in that: The homogenization treatment is carried out at 500° C. for 12 hours.
3. The method for improving the toughness of ZL205A alloy according to claim 1, characterized in that: The preheating temperature of ZL205A alloy is 30℃ higher than the preheating temperature of extrusion die, and the preheating time is 30min.
4. The method for improving the strength and toughness of ZL205A alloy according to claim 1, characterized in that: The extrusion speed is 4 mm / s, and the extrusion temperature is 350°C.
5. The method for improving the strength and toughness of ZL205A alloy according to any one of claims 1 to 4, characterized in that: Also includes: S4: The ZL205A alloy treated by S3 is subjected to solution treatment and aging treatment in sequence, and then air-cooled to room temperature.
6. The method for improving the strength and toughness of ZL205A alloy according to claim 5, characterized in that: The solution treatment is carried out at 500-540°C for 14 hours, and the aging treatment is carried out at 175°C for 4 hours.
7. The method for improving the strength and toughness of ZL205A alloy according to claim 1, characterized in that: Rare earth elements are added to the ZL205A alloy before homogenization treatment.
8. The method for improving the strength and toughness of ZL205A alloy according to claim 7, characterized in that: The rare earth element is Sc.
9. The method for improving the strength and toughness of ZL205A alloy according to claim 8, characterized in that: The added amount of Sc is 0.05-0.2 wt % of the ZL205A alloy.
10. The method for improving the strength and toughness of ZL205A alloy according to any one of claims 7 to 9, characterized in that: The steps for adding rare earth elements are: S1: Add ZL205A alloy and rare earth elements into a resistance furnace for melting and heat to 740℃; S2: Degassing with argon, then continue heating to 760°C, refining and keeping the temperature for 20 minutes; S3: Pour the melt into a metal mold and cool it.