Cobalt removal method for polycrystalline diamond compact
Through three-stage impregnation method and ultrasonic technology, the problem of low decobalt removal efficiency of polycrystalline diamond composite sheets is solved, and the decobalt removal efficiency and material performance are improved.
Patent Information
- Application Number
- CN202411083917.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
The existing method of decobalt decobalt of polycrystalline diamond composite sheets is inefficient, and the overall decobalt decobalt time is long, resulting in a decrease in efficiency.
The three-stage impregnation method is used to combine ultrasonic technology, and by configuring a composite acid solution and an ultrasonic generator, rapid impregnation, constant temperature impregnation and cooling impregnation are carried out to control the concentration and temperature of the acid and improve the decobalt removal efficiency.
The removal efficiency of cobalt element is significantly improved, and the wear resistance and resistivity of polycrystalline diamond composite sheet is enhanced.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of diamonds, and more specifically, to a method for removing cobalt from a polycrystalline diamond composite sheet. Background Art
[0002] Diamond is a superhard material with very high hardness, mainly used to make various diamond tools, such as grinding tools, wire drawing dies, cutting tools and drilling tools. The cobalt removal technology of composite sheets is to remove the cobalt element in the diamond layer. The cobalt element is a binder added when sintering the composite sheet, and it is macroscopically uniformly distributed in the diamond. Acid melting or electrolysis is usually adopted. The reason for removing the cobalt element is that when the polycrystalline diamond composite sheet is working, the composite sheet and the rock generate heat due to friction, and its own temperature will continue to increase. However, the thermal expansion coefficients of carbon elements (artificial diamonds) and cobalt elements are different. When working, the volume will increase with the increase of temperature, thereby causing an increase in internal stress and causing the destruction of the composite sheet. Cobalt removal plays an important role in polycrystalline diamond composite sheets. When the existing cobalt removal method of polycrystalline diamond composite sheets is working, the overall cobalt removal time is long, and the deeper the cobalt removal depth, the longer the cobalt removal time, resulting in low overall efficiency. For this reason, we propose a cobalt removal method for polycrystalline diamond composite sheets. Summary of the invention
[0003] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for removing cobalt from a polycrystalline diamond composite sheet.
[0004] A method for removing cobalt from a polycrystalline diamond composite sheet comprises the following steps:
[0005] S1. Prepare the decobalt solution:
[0006] (1) Prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L
[0007] (2) mixing a composite acid solution A having a mass concentration of 50 g / L to 160 g / L with a composite acid solution B having a mass concentration of 3 g / L to 40 g / L to obtain a decobaltized solution;
[0008] S2, decobalting: immerse the polycrystalline diamond composite sheet in the prepared decobalting solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and adopt a three-stage impregnation method. In the rapid impregnation stage, first quickly heat up to 80°C to 90°C, and then increase the pressure to 1.2Mpa constant pressure, and immerse for 12 hours. In the constant temperature impregnation stage, slowly adjust the impregnation temperature to 100°C to 130°C, 2.1Mpa constant pressure, and immerse for 20 to 34 hours. In the cooling impregnation stage, gradually reduce the impregnation temperature to 80°C and keep the temperature constant for 10 hours, and then gradually cool to room temperature, and the impregnation ends;
[0009] S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged;
[0010] S4, drying: drying the rinsed polycrystalline diamond composite sheet.
[0011] Preferably, the composite acid solution A is composed of the following parts by weight: 3-4 parts of sulfuric acid solution, 8-12 parts of hypochlorous acid, 7-9 parts of sulfinic acid, and 4-7 parts of hydrochloric acid.
[0012] Preferably, the composite acid solution B is composed of the following parts by weight: 7 to 9 parts of citric acid, 3 to 8 parts of hydrobromic acid, and 6 to 13 parts of nitric acid.
[0013] Preferably, the frequency of the ultrasonic generator is 30-90 KHZ.
[0014] Preferably, in the three-stage impregnation method, the frequency of the ultrasonic generator in the rapid impregnation stage is 30-40 KHZ, the frequency of the ultrasonic generator in the constant temperature impregnation stage is 70-90 KHZ, and the frequency of the ultrasonic generator in the cooling impregnation stage is 50-60 KHZ.
[0015] Technical effects and advantages of the present invention:
[0016] 1. The present invention performs a rapid impregnation section, a constant temperature impregnation section and a cooling impregnation section on the polycrystalline diamond composite sheet during the cobalt removal process. The whole process adopts a three-stage impregnation method, which can effectively remove the cobalt in the polycrystalline diamond and improve the efficiency. In addition, an ultrasonic rod generator is used in the whole process to make the polycrystalline diamond composite sheet fully contact with the cobalt removal solution, effectively improving the cobalt removal efficiency.
[0017] 2. The present invention adopts a three-stage impregnation method, which can effectively control the acid concentration, leaching temperature and time in the decobalting solution, so that the wear resistance and resistivity of the decobalting polycrystalline diamond composite sheet are greatly improved. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0019] Example 1
[0020] A method for removing cobalt from a polycrystalline diamond composite sheet comprises the following steps:
[0021] S1. Prepare the decobalt solution:
[0022] (1) Select 3 parts of sulfuric acid solution, 8 parts of hypochlorous acid, 7 parts of sulfinic acid and 4 parts of hydrochloric acid to prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; select 7 parts of citric acid, 3 parts of hydrobromic acid and 6 to 13 parts of nitric acid to prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L
[0023] (2) mixing a composite acid solution A having a mass concentration of 50 g / L and a composite acid solution B having a mass concentration of 3 g / L to obtain a decobaltized solution;
[0024] S2. Cobalt removal: Immerse the polycrystalline diamond composite sheet with a composite layer thickness of 2 mm into the prepared cobalt removal solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and externally heat the reactor, while using a three-stage immersion method:
[0025] (1) Rapid immersion stage: firstly, the temperature is quickly raised to 80°C, the pressure is automatically raised to a constant pressure of 1.2 MPa, and the frequency of the ultrasonic rod generator is set to 30 KHZ, and the immersion is continued for 12 hours;
[0026] (2) Constant temperature immersion stage: slowly adjust the immersion temperature to 100°C and the constant pressure to 2.1 MPa, and set the frequency of the ultrasonic rod generator to 70 KHZ for immersion for 20 to 34 hours;
[0027] (3) Cooling and immersion stage: the frequency of the ultrasonic rod generator is set to 50KHZ, and the immersion temperature is gradually reduced. After the immersion temperature drops to 80°C, the temperature is kept constant for 10 hours. After the time is up, the heating is stopped. When the immersion temperature drops to 40°C, the ultrasonic rod generator stops working. The immersion temperature is cooled to room temperature, and the immersion is completed.
[0028] S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged;
[0029] S4, drying: drying the rinsed polycrystalline diamond composite sheet.
[0030] Example 2
[0031] A method for removing cobalt from a polycrystalline diamond composite sheet comprises the following steps:
[0032] S1. Prepare the decobalt solution:
[0033] (1) Select 3 parts of sulfuric acid solution, 10 parts of hypochlorous acid, 8 parts of sulfinic acid and 5 parts of hydrochloric acid to prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; select 8 parts of citric acid, 5 parts of hydrobromic acid and 9 parts of nitric acid to prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L
[0034] (2) mixing a composite acid solution A having a mass concentration of 80 g / L and a composite acid solution B having a mass concentration of 20 g / L to obtain a decobaltized solution;
[0035] S2. Cobalt removal: Immerse the polycrystalline diamond composite sheet with a composite layer thickness of 2 mm into the prepared cobalt removal solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and externally heat the reactor, while using a three-stage immersion method:
[0036] (1) Rapid immersion stage: firstly, the temperature is rapidly raised to 85°C, the pressure is automatically raised to a constant pressure of 1.2 MPa, and the frequency of the ultrasonic rod generator is set to 35 KHZ, and the immersion is continued for 12 hours;
[0037] (2) Constant temperature immersion stage: slowly adjust the immersion temperature to 115°C and the constant pressure to 2.1 MPa, and set the frequency of the ultrasonic rod generator to 80 KHZ for immersion for 20 to 34 hours;
[0038] (3) Cooling and immersion stage: the frequency of the ultrasonic rod generator is set to 55KHZ, and the immersion temperature is gradually reduced. After the immersion temperature drops to 80°C, the temperature is kept constant for 10 hours. After the time is up, the heating is stopped. When the immersion temperature drops to 40°C, the ultrasonic rod generator stops working. The immersion temperature is cooled to room temperature, and the immersion is completed.
[0039] S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged;
[0040] S4, drying: drying the rinsed polycrystalline diamond composite sheet.
[0041] Example 3
[0042] A method for removing cobalt from a polycrystalline diamond composite sheet comprises the following steps:
[0043] S1. Prepare the decobalt solution:
[0044] (1) Select 4 parts of sulfuric acid solution, 11 parts of hypochlorous acid, 8 parts of sulfinic acid and 6 parts of hydrochloric acid to prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; select 8 parts of citric acid, 6 parts of hydrobromic acid and 11 parts of nitric acid to prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L
[0045] (2) mixing a composite acid solution A having a mass concentration of 140 g / L and a composite acid solution B having a mass concentration of 30 g / L to obtain a decobaltized solution;
[0046] S2. Cobalt removal: Immerse the polycrystalline diamond composite sheet with a composite layer thickness of 2 mm into the prepared cobalt removal solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and externally heat the reactor, while using a three-stage immersion method:
[0047] (1) Rapid immersion stage: firstly, the temperature is rapidly raised to 90°C, the pressure is automatically raised to a constant pressure of 1.2 MPa, and the frequency of the ultrasonic rod generator is set to 40 KHZ, and the immersion is continued for 12 hours;
[0048] (2) Constant temperature immersion stage: slowly adjust the immersion temperature to 120°C and the constant pressure to 2.1 MPa, and set the frequency of the ultrasonic rod generator to 90 KHZ for immersion for 20 to 34 hours;
[0049] (3) Cooling and immersion stage: the frequency of the ultrasonic rod generator is set to 60KHZ, and the immersion temperature is gradually reduced. After the immersion temperature drops to 80°C, the temperature is kept constant for 10 hours. After the time is up, the heating is stopped. When the immersion temperature drops to 40°C, the ultrasonic rod generator stops working. The immersion temperature is cooled to room temperature, and the immersion is completed.
[0050] S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged;
[0051] S4, drying: drying the rinsed polycrystalline diamond composite sheet.
[0052] Example 4
[0053] A method for removing cobalt from a polycrystalline diamond composite sheet comprises the following steps:
[0054] S1. Prepare the decobalt solution:
[0055] (1) Select 4 parts of sulfuric acid solution, 12 parts of hypochlorous acid, 9 parts of sulfinic acid and 7 parts of hydrochloric acid to prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; select 9 parts of citric acid, 8 parts of hydrobromic acid and 13 parts of nitric acid to prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L
[0056] (2) mixing a composite acid solution A having a mass concentration of 160 g / L with a composite acid solution B having a mass concentration of 40 g / L to obtain a decobaltized solution;
[0057] S2. Cobalt removal: Immerse the polycrystalline diamond composite sheet with a composite layer thickness of 1.5 mm into the prepared cobalt removal solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and externally heat the reactor, while using a three-stage immersion method:
[0058] (1) Rapid immersion stage: firstly, the temperature is rapidly raised to 90°C, the pressure is automatically raised to a constant pressure of 1.2 MPa, and the frequency of the ultrasonic rod generator is set to 40 KHZ, and the immersion is continued for 12 hours;
[0059] (2) Constant temperature immersion stage: slowly adjust the immersion temperature to 130°C and the constant pressure to 2.1 MPa, and set the frequency of the ultrasonic rod generator to 90 KHZ for immersion for 20 to 34 hours;
[0060] (3) Cooling and immersion stage: the frequency of the ultrasonic rod generator is set to 60KHZ, and the immersion temperature is gradually reduced. After the immersion temperature drops to 80°C, the temperature is kept constant for 10 hours. After the time is up, the heating is stopped. When the immersion temperature drops to 40°C, the ultrasonic rod generator stops working. The immersion temperature is cooled to room temperature, and the immersion is completed.
[0061] S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged;
[0062] S4, drying: drying the rinsed polycrystalline diamond composite sheet.
[0063] Example 5
[0064] The polycrystalline diamond composite sheets obtained in Examples 1, 2, 3 and 4 were selected and placed in a laser heating device. The temperature in the laser heating device was then raised to between 900° C. and 1300° C. The polycrystalline diamond composite sheets were placed in the laser heating device for 2 minutes to 24 hours to break the decobaltized layer into fragments. At the same time, the entire diamond layer also fell off the cemented carbide substrate. Finally, the thickness of each fragment was measured with a micrometer or a vernier caliper to obtain the decobaltization depth, and the following table was obtained:
[0065] Composite layer thickness (mm) Cobalt removal thickness (mm) Cobalt content after decobalting (wt%) Example 1 2 1.19 0.39 Example 2 2 1.03 0.41 Example 3 2 1.21 0.38 Example 4 1.5 1.05 0.32
[0066] The invention can effectively control the concentration of acid in the decobalting solution, the leaching temperature and the time by performing a rapid immersion section, a constant temperature immersion section and a cooling immersion section on the polycrystalline diamond composite sheet during the decobalting process, and can effectively remove the cobalt in the polycrystalline diamond and improve the efficiency.
[0067] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for removing cobalt from a polycrystalline diamond composite sheet, characterized in that: The steps include: S1. Prepare the cobalt removal solution: (1) Prepare a composite acid solution A with a mass concentration of 50 g / L to 160 g / L; prepare a composite acid solution B with a mass concentration of 3 g / L to 40 g / L (2) mixing a composite acid solution A having a mass concentration of 50 g / L to 160 g / L with a composite acid solution B having a mass concentration of 3 g / L to 40 g / L to obtain a decobaltized solution; S2, decobalting: immerse the polycrystalline diamond composite sheet in the prepared decobalting solution, add an ultrasonic rod generator into the reaction tank, seal the reactor, start the ultrasonic rod generator, and adopt a three-stage impregnation method. In the rapid impregnation stage, first quickly heat up to 80°C to 90°C, and then increase the pressure to 1.2Mpa constant pressure, and immerse for 12 hours. In the constant temperature impregnation stage, slowly adjust the impregnation temperature to 100°C to 130°C, 2.1Mpa constant pressure, and immerse for 20 to 34 hours. In the cooling impregnation stage, gradually reduce the impregnation temperature to 80°C and keep the temperature constant for 10 hours, and then gradually cool to room temperature, and the impregnation ends; S3, rinsing: the polycrystalline diamond composite sheet is fished out and rinsed clean, and the water used to rinse the composite sheet is treated before being discharged; S4, drying: drying the rinsed polycrystalline diamond composite sheet.
2. The method for removing cobalt from a polycrystalline diamond compact according to claim 1, characterized in that: The composite acid solution A is composed of the following parts by weight: 3-4 parts of sulfuric acid solution, 8-12 parts of hypochlorous acid, 7-9 parts of sulfinic acid, and 4-7 parts of hydrochloric acid.
3. The method for removing cobalt from a polycrystalline diamond compact according to claim 1, characterized in that: The composite acid solution B is composed of the following parts by weight: 7 to 9 parts of citric acid, 3 to 8 parts of hydrobromic acid, and 6 to 13 parts of nitric acid.
4. The method for removing cobalt from a polycrystalline diamond compact according to claim 1, characterized in that: The frequency of the ultrasonic generator is 30-90 KHZ.
5. The method for removing cobalt from a polycrystalline diamond compact according to claim 4, characterized in that: In the three-stage impregnation method, the frequency of the ultrasonic generator in the rapid impregnation stage is 30-40KHZ, in the constant temperature impregnation stage, the frequency of the ultrasonic generator is 70-90KHZ, and in the cooling impregnation stage, the frequency of the ultrasonic generator is 50-60KHZ.