Integrated water electrolysis hydrogen production electrode and preparation method and application thereof
Through the integrated design of electrolytic water hydrogen production electrode, the integrated conductive substrate, fluid diffusion layer and catalytic electrode layer, the problems of high current density and high energy consumption in existing electrode technologies are solved, and the alkaline electrolytic water hydrogen production technology is improved and Simplified assembly.
Patent Information
- Application Number
- CN202411079789.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The electrode technology of existing alkaline electrolytic cells has problems such as unbearable high current density, high energy consumption, high production costs, and failure to fully combine catalytic reactions and fluid diffusion, resulting in increased assembly complexity.
An integrated electrolytic hydrogen production electrode is designed, and the conductive substrate, fluid diffusion layer and catalytic electrode layer are stacked to reduce contact resistance, reduce electrolytic voltage and energy consumption, and simplify assembly complexity.
The alkaline electrolytic hydrogen production technology has been improved, the electrolytic voltage and energy consumption has been reduced, the electrode structure has been simplified, and the electrolytic reaction efficiency has been improved.
Smart Images

Figure CN118979267A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of hydrogen production electrodes, and in particular relates to an integrated water electrolysis hydrogen production electrode and a preparation method and application thereof. Background Art
[0002] In recent years, the global environment has continued to deteriorate due to the greenhouse effect, and the frequency and destructive power of extreme weather have also been increasing. In order to curb the further escalation of this deterioration, it is necessary to use cleaner new energy to change this situation. Hydrogen energy, especially green hydrogen based on solar and wind power generation, has been widely valued as a clean energy without any carbon emissions. Major countries, including my country, have included hydrogen energy in their energy strategic system. Under widespread attention, related technologies have also made great progress. As the core component for converting electricity to hydrogen energy, alkaline electrolyzers have received more and more attention in recent years. The single-cell capacity of electrolyzers has been continuously expanding, and the overall shipments have increased exponentially. Related products are in short supply. In contrast to the hot market demand, the production technology of alkaline electrolyzers, especially the electrode technology, has made relatively weak progress. It is still in the traditional Raney nickel spraying method. The electrode is difficult to withstand high current density, resulting in high electrolysis energy consumption. In addition, the preparation process uses high-energy-consuming methods such as plasma spraying and electroplating, and the production cost is high. Furthermore, the existing electrode structure does not fully combine the catalytic reaction and fluid diffusion, and adopts the method that the electrode is the electrode and the diffusion layer is the diffusion layer, which increases the complexity of assembly.
[0003] Therefore, it is urgent to design a new type of water electrolysis hydrogen production electrode to improve the alkaline water electrolysis hydrogen production technology. Summary of the invention
[0004] In view of the deficiencies of the prior art, the purpose of the present invention is to provide an integrated water electrolysis hydrogen production electrode and its preparation method and application. The present invention provides an integrated water electrolysis hydrogen production electrode. After the electrode is assembled into the electrolytic cell chamber, the conductive substrate contacts the bipolar plate of the chamber to realize the conduction of current from the bipolar plate to the electrode. The fluid diffusion layer provides electrolyte for the electrolysis reaction while collecting the generated hydrogen or oxygen to form a gas-liquid channel and discharge it from the chamber. The catalytic electrode layer is the place for electrochemical reaction of electrolysis, and the water molecules in the electrolyte are electrolyzed into hydrogen and oxygen under the action of the current. In summary, the present invention integrates the conductive substrate, the fluid diffusion layer and the catalytic electrode layer into one, reduces the contact resistance of each component of the original structure, further reduces the hydrogen production electrolysis voltage, reduces the energy consumption of hydrogen production, and also reduces the number of components and assembly complexity, thus realizing a leap in alkaline water electrolysis hydrogen production technology.
[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides an integrated water electrolysis hydrogen production electrode, wherein the integrated water electrolysis hydrogen production electrode comprises a conductive substrate, a fluid diffusion layer and a catalytic electrode layer which are stacked.
[0007] The present invention provides an integrated electrolytic water hydrogen production electrode. After the electrode is assembled into the electrolytic cell chamber, the conductive substrate contacts the bipolar plate of the chamber to realize the conduction of current from the bipolar plate to the electrode. The fluid diffusion layer provides electrolyte for the electrolysis reaction while collecting the generated hydrogen or oxygen to form a gas-liquid channel and discharge it from the chamber. The catalytic electrode layer is the place for electrochemical reaction of electrolysis, and the water molecules in the electrolyte are electrolyzed into hydrogen and oxygen under the action of the current. In summary, the present invention integrates the conductive substrate, the fluid diffusion layer and the catalytic electrode layer into one, reduces the contact resistance of each component of the original structure, further reduces the hydrogen electrolysis voltage, reduces the energy consumption of hydrogen production, and also reduces the number of components and assembly complexity, thus realizing a leap in alkaline water electrolysis hydrogen production technology.
[0008] And / or, the conductive substrate includes a nickel plate and / or a nickel-plated steel plate.
[0009] In the present invention, the conductive substrate mainly plays a supporting role, plays a role in contacting with the bipolar plate to conduct current after the electrode is formed, and serves as a carrier of the slurry during the electrode preparation process.
[0010] And / or, the thickness of the conductive substrate is 0.05-0.1 mm, for example, 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm or 0.1 mm.
[0011] And / or, the fluid transmitted by the fluid diffusion layer includes gas and liquid.
[0012] And / or, the fluid diffusion layer is a porous structure.
[0013] And / or, the porosity of the fluid diffusion layer is 70-98%, for example, 70%, 75%, 78%, 80%, 86%, 90%, 95% or 98%, etc.
[0014] And / or, the average pore size of the fluid diffusion layer is 2-4 mm, for example, 2 mm, 2.1 mm, 2.35 mm, 2.8 mm, 3 mm, 3.5 mm or 4 mm.
[0015] In the present invention, if the average pore size of the fluid diffusion layer is too small, the fluid flow impedance increases, resulting in a decrease in the fluid flow capacity, and a greater pressure is required to drive the fluid flow. In severe cases, local eddy currents may occur, resulting in the inability to supply liquid to the electrode reaction zone in time, or the inability to discharge gas from the reaction zone in time, thereby affecting the efficiency of the electrolysis reaction.
[0016] And / or, the raw materials for preparing the fluid diffusion layer include metal powder, a first foaming agent and a first binder, and the mass ratio of the metal powder, the first foaming agent and the first binder is (80-95):(0.1-5):(0.5-5), wherein the selection range of the metal powder "80-95" can be, for example, 80, 85, 90 or 95, etc., the selection range of the first foaming agent "0.1-5" can be, for example, 0.1, 0.5, 1, 2, 3, 4 or 5, etc., and the selection range of the first binder "0.5-5" can be, for example, 0.5, 1, 2, 3, 4 or 5, etc.
[0017] And / or, the catalytic electrode layer is a porous catalytic electrode.
[0018] And / or, the porosity of the porous catalytic electrode is 80-95%, for example, it can be 80%, 85%, 88%, 90% or 95%, etc.
[0019] And / or, the average pore size of the porous catalytic electrode is 5-100 μm, for example, 5 μm, 8 μm, 15 μm, 20 μm, 30 μm, 42 μm, 60 μm, 75 μm or 100 μm, etc.
[0020] In the present invention, if the average pore size of the porous catalytic electrode is too large, the specific surface area of the catalytic electrode will be too small, and the catalytic ability will decrease. On the contrary, if the pore size is too small, it will be unfavorable for the transmission of alkali solution and it will be difficult to form a gas-liquid-solid three-phase interface, resulting in the inability to sustain the electrolysis of water reaction.
[0021] And / or, the specific surface area of the porous catalytic electrode is 80-300m 2 / g, for example, it can be 80m 2 / g, 88m 2 / g, 150m 2 / g, 220m 2 / g, 250m 2 / g or 300m 2 / g, etc.
[0022] And / or, the raw materials for preparing the catalytic electrode layer include an alloy material, a second foaming agent and a second binder, and the mass ratio of the alloy material, the second foaming agent and the second binder is (80-95):(0.1-5):(0.5-5), wherein the selection range of the alloy material "80-95" can be, for example, 80, 85, 90 or 95, etc., the selection range of the second foaming agent "0.1-5" can be, for example, 0.1, 0.5, 1, 2, 3, 4 or 5, etc., and the selection range of the second binder "0.5-5" can be, for example, 0.5, 1, 2, 3, 4 or 5, etc.
[0023] And / or, the thickness ratio of the fluid diffusion layer transport layer and the catalytic electrode layer is (3-6):(0.5-1.5), wherein the selection range of the fluid diffusion layer transport layer "3-6" can be, for example, 3, 3.2, 3.5, 3.8, 4, 4.5, 5, 5.5 or 6, and the selection range of the catalytic electrode layer "0.5-1.5" can be, for example, 0.5, 0.8, 1.03, 1.1, 1.3 or 1.5, etc.
[0024] In the present invention, if the thickness ratio of the fluid diffusion layer, the transmission layer and the catalytic electrode layer is too small, the catalytic layer will be too thick or the transmission layer will be too small, which will cause the gas-liquid transmission distance in the catalytic layer to be too long, increase the transmission resistance, and be unfavorable for the electrolysis reaction; if the thickness ratio of the fluid diffusion layer, the transmission layer and the catalytic electrode layer is too large, the transmission layer will be too large, which will increase the gas-liquid transmission distance and reduce the uniformity of fluid distribution. At the same time, due to the increase in distance, the electron transmission distance will increase, the resistance will increase, which is not conducive to reducing the energy consumption of electrolysis.
[0025] In a second aspect, the present invention provides a method for preparing the integrated water electrolysis hydrogen production electrode as described in the first aspect, the preparation method comprising the following steps:
[0026] Providing a conductive substrate, coating the surface of the conductive substrate to be coated with a slurry for preparing a fluid diffusion layer, and drying to form a fluid diffusion precursor layer to obtain a semi-finished electrode;
[0027] The preparation slurry of the catalytic electrode layer is coated on the surface of the fluid diffusion precursor layer, and after drying, a catalytic electrode precursor layer is formed, which is then sintered and activated to obtain the integrated water electrolysis hydrogen production electrode.
[0028] And / or, the slurry for preparing the fluid diffusion layer includes metal powder, a first foaming agent, a first binder and water.
[0029] And / or, the metal powder is nickel powder or nickel-based alloy powder.
[0030] And / or, the slurry for preparing the catalytic electrode layer includes an alloy material, a second foaming agent, a second binder and water.
[0031] And / or, the alloy material includes a binary alloy, a ternary alloy or a multi-element alloy, and the metal species of the multi-element alloy are ≥4, such as a quaternary alloy, a quinary alloy or a hexa-element alloy.
[0032] And / or, the alloy material further includes an alloy material doped with a precious metal.
[0033] And / or, the binary alloy includes any one of Raney nickel alloy, nickel-zinc alloy or nickel-iron alloy, or a combination of at least two thereof.
[0034] And / or, the ternary alloy comprises a nickel-aluminum-molybdenum alloy.
[0035] And / or, the multi-element alloy includes nickel-aluminum-zinc-molybdenum-iron-platinum alloy.
[0036] And / or, the first blowing agent and the second blowing agent independently comprise carbonates.
[0037] And / or, the carbonate comprises potassium carbonate.
[0038] And / or, the first binder and the second binder independently include carboxymethyl cellulose and / or styrene-butadiene rubber.
[0039] And / or, the sintering process is carried out in a reducing atmosphere.
[0040] In the present invention, the purpose of limiting the sintering process to be carried out in a reducing atmosphere is to ensure that the metal is not oxidized during the sintering process. Under laboratory conditions, it can be completed in a sintering furnace, and under mass production conditions, it is usually completed in a vertical long tubular sintering furnace.
[0041] And / or, the gas in the reducing atmosphere includes an inert gas and hydrogen.
[0042] And / or, in the reducing atmosphere, the volume fraction of hydrogen is 60-80%, for example, 60%, 62%, 65%, 70% or 80%.
[0043] And / or, the sintering temperature is 1200-1400°C, for example, it can be 1200°C, 1250°C, 1300°C, 1350°C or 1400°C.
[0044] In the present invention, if the sintering temperature is too low, the metal powder cannot be partially melted, so that the powders cannot be fused into a whole, resulting in difficulty in molding or low strength and high resistance after molding, and the material cannot be used; if the sintering temperature is too high, the powder will be completely melted, and large pieces of metal material will be formed after cooling, which will lose the designed porous material shape and the catalytic surface area, resulting in material failure.
[0045] It should be noted that the present invention does not limit the sintering time. For example, it can be 5 min-20 min, such as 5 min, 10 min, 15 min or 20 min.
[0046] And / or, the specific steps of the activation include:
[0047] The sintered product is placed in an activation solution for activation.
[0048] In the present invention, activation can dissolve the metal ions in the catalytic electrode layer, thereby generating a large number of pores, significantly increasing the surface area of the catalytic electrode layer, and the prepared catalytic electrode layer has a good catalytic effect on water electrolysis. Under laboratory conditions, the electrode can be immersed in an activation solution; and in mass production, a multi-slot structure is used to realize the automated production of activation solution immersion, cleaning, drying and other processes.
[0049] And / or, the activation solution includes KOH solution.
[0050] And / or, the activation temperature is 50-80°C, for example, 50°C, 52°C, 55°C, 60°C, 70°C, 75°C or 80°C.
[0051] In the present invention, if the activation temperature is too low, the activation time will be long and the efficiency will be low, affecting the production progress; if the activation temperature is too high, the activation time will be difficult to control, and over-activation with excessive metal dissolution will easily occur, affecting the performance of the electrode.
[0052] And / or, the preparation method comprises the following steps:
[0053] (1) stirring and mixing metal powder, a first foaming agent, a first binder and water in a mass ratio of (80-95):(0.1-5):(0.5-5):(5-15) to obtain a slurry for preparing a fluid diffusion layer;
[0054] The alloy material, the second foaming agent, the second binder and water are stirred and mixed in a mass ratio of (80-95):(0.1-5):(0.5-5):(5-15) to obtain a slurry for preparing a catalytic electrode layer;
[0055] (2) coating the prepared slurry of the fluid diffusion layer on the surface to be coated of the conductive substrate, and forming a fluid diffusion precursor layer after drying to obtain a semi-finished electrode;
[0056] Wherein, the drying temperature is less than 120°C (for example, it can be 110°C, 100°C, 90°C or 80°C, etc.), and the drying time is less than 10min (for example, it can be 8min, 6min, 4min or 2min, etc.);
[0057] (3) coating the surface of the fluid diffusion precursor layer with a slurry for preparing the catalytic electrode layer, drying it to form a catalytic electrode precursor layer, and then sintering it at 1200-1400°C under the protection of a reducing atmosphere, so that the conductive substrate, the fluid diffusion precursor layer and the catalytic electrode precursor layer are partially melted and integrated into one, and then placed in an activation solution with a temperature of 50-80°C for activation, thereby preparing the integrated water electrolysis hydrogen production electrode.
[0058] In a third aspect, the present invention provides an application of the integrated water electrolysis hydrogen production electrode as described in the first aspect, wherein the integrated water electrolysis hydrogen production electrode is applied in the field of water electrolysis.
[0059] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] The present invention provides an integrated water electrolysis hydrogen production electrode. After the electrode is assembled into the electrolytic cell chamber, the conductive substrate contacts the bipolar plate of the chamber to realize the conduction of current from the bipolar plate to the electrode. The fluid diffusion layer provides electrolyte for the electrolysis reaction while collecting the generated hydrogen or oxygen to form a gas-liquid channel and discharge it from the chamber. The catalytic electrode layer is the place for electrochemical reaction of electrolysis, and the water molecules in the electrolyte are electrolyzed into hydrogen and oxygen under the action of the current. In summary, the present invention integrates the conductive substrate, the fluid diffusion layer and the catalytic electrode layer into one, reduces the contact resistance of each component of the original structure, reduces the number of components, reduces the complexity of assembly, and realizes a leap in the alkaline water electrolysis hydrogen production technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is a schematic diagram of the structure of the integrated water electrolysis hydrogen production electrode prepared in Example 1 of the present invention.
[0063] Among them, 1-conductive substrate; 2-fluid diffusion layer; 3-catalytic electrode layer. DETAILED DESCRIPTION
[0064] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0065] Example 1
[0066] This embodiment provides an integrated water electrolysis hydrogen production electrode, and its structural schematic diagram is as follows Figure 1 As shown, the integrated water electrolysis hydrogen production electrode comprises a conductive substrate 1, a fluid diffusion layer 2 and a catalytic electrode layer 3 which are stacked;
[0067] The conductive substrate 1 is a nickel plate with a thickness of 0.1 mm;
[0068] The fluid diffusion layer 2 is a porous structure with a porosity of 92% and an average pore size of 2.7 mm; the raw materials for preparing the fluid diffusion layer 2 include nickel powder, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the nickel powder, potassium carbonate and carboxymethyl cellulose is 94:4:2;
[0069] The catalytic electrode layer 3 is a porous catalytic electrode having a porosity of 82%, an average pore size of 50 μm, and a specific surface area of 220 m 2 / g; the raw materials for preparing the catalytic electrode layer 3 include Raney nickel alloy, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the Raney nickel alloy, potassium carbonate and carboxymethyl cellulose is 94:4:2;
[0070] The thickness ratio of the fluid diffusion layer transport layer 2 and the catalytic electrode layer 3 is 4:1.
[0071] This embodiment also provides a method for preparing the above-mentioned integrated water electrolysis hydrogen production electrode, the preparation method comprising the following steps:
[0072] (1) nickel powder and potassium carbonate are mechanically mixed using a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during stirring and mixing is controlled to be 30° C. and the time is 120 min by using a double-layer slurry barrel and passing cooling water in the gap between the double layers, thereby obtaining a preparation slurry for the fluid diffusion layer 3; the mass ratio of nickel powder, potassium carbonate, carboxymethyl cellulose and water is 82.72:3.52:1.76:12;
[0073] The Raney nickel alloy and potassium carbonate are mechanically mixed using a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during stirring and mixing is controlled to be 30° C. and the time is 120 minutes by using a double-layer slurry barrel and passing cooling water in the gap between the double layers to obtain a slurry for preparing the catalytic electrode layer 4; the mass ratio of the Raney nickel alloy, potassium carbonate, carboxymethyl cellulose and water is 82.72:3.52:1.76:12;
[0074] (2) coating the prepared slurry of the fluid diffusion layer 2 on the surface to be coated of the conductive substrate 1, removing moisture after drying in an oven, forming a fluid diffusion precursor layer, and obtaining a semi-finished electrode;
[0075] Among them, the drying temperature is 110℃ and the drying time is 5min;
[0076] (3) coating the surface of the fluid diffusion precursor layer with the slurry for preparing the catalytic electrode layer 3, removing moisture after drying in an oven at a temperature of 110° C. for 5 min to form a catalytic electrode precursor layer, and then sintering at 1300° C. under the protection of a reducing atmosphere for 10 min to allow the conductive substrate, the fluid diffusion precursor layer and the catalytic electrode precursor layer to be partially melted and integrated, and then placed in a KOH solution at a temperature of 60° C. for activation to prepare the integrated water electrolysis hydrogen production electrode;
[0077] The gas in the reducing atmosphere includes nitrogen and hydrogen, and the volume fraction of hydrogen is 75%.
[0078] Example 2
[0079] This embodiment provides an integrated water electrolysis hydrogen production electrode, the integrated water electrolysis hydrogen production electrode comprising a conductive substrate, a fluid diffusion layer and a catalytic electrode layer stacked;
[0080] The conductive substrate is a nickel plate with a thickness of 0.1 mm;
[0081] The fluid diffusion layer is a porous structure with a porosity of 94% and an average pore size of 3 mm; the raw materials for preparing the fluid diffusion layer include nickel powder, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the nickel powder, potassium carbonate and carboxymethyl cellulose is 93:5:2;
[0082] The catalytic electrode layer is a porous catalytic electrode, the porosity of the porous catalytic electrode is 84%, the average pore size is 60 μm, and the specific surface area is 200 m 2 / g; the raw materials for preparing the catalytic electrode layer include Raney nickel alloy, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the Raney nickel alloy, potassium carbonate and carboxymethyl cellulose is 93:5:2;
[0083] The thickness ratio of the fluid diffusion layer, the transport layer and the catalytic electrode layer is 4:1.
[0084] This embodiment also provides a method for preparing the above-mentioned integrated water electrolysis hydrogen production electrode, the preparation method comprising the following steps:
[0085] (1) nickel powder and potassium carbonate are mechanically mixed using a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during stirring and mixing is controlled to be 30° C. and the time is 120 min by using a double-layer slurry barrel and passing cooling water in the gap between the double layers to obtain a preparation slurry for a fluid diffusion layer; the mass ratio of nickel powder, potassium carbonate, carboxymethyl cellulose and water is 80.91:4.35:1.74:13;
[0086] The Raney nickel alloy and potassium carbonate are mechanically mixed by a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during the stirring and mixing is controlled to be 30° C. and the time is 120 minutes by using a double-layer slurry barrel and passing cooling water in the gap between the double layers to obtain a slurry for preparing a catalytic electrode layer; the mass ratio of the Raney nickel alloy, potassium carbonate, carboxymethyl cellulose and water is 80.91:4.35:1.74:13;
[0087] (2) coating the prepared slurry of the fluid diffusion layer on the surface to be coated of the conductive substrate, drying it in an oven to remove moisture, forming a fluid diffusion precursor layer, and obtaining a semi-finished electrode;
[0088] Among them, the drying temperature is 80℃ and the drying time is 8min;
[0089] (3) coating the surface of the fluid diffusion precursor layer with the slurry for preparing the catalytic electrode layer, drying it in an oven to remove moisture, the drying temperature is 80° C., the drying time is 8 min, to form a catalytic electrode precursor layer, and then sintering it at 1200° C. under the protection of a reducing atmosphere, the constant temperature time is 20 min, so that the conductive substrate, the fluid diffusion precursor layer and the catalytic electrode precursor layer are partially melted and integrated, and then placed in a KOH solution at a temperature of 60° C. for activation, to prepare the integrated water electrolysis hydrogen production electrode;
[0090] The gas in the reducing atmosphere includes nitrogen and hydrogen, and the volume fraction of hydrogen is 75%.
[0091] Example 3
[0092] This embodiment provides an integrated water electrolysis hydrogen production electrode, the integrated water electrolysis hydrogen production electrode comprising a conductive substrate, a fluid diffusion layer and a catalytic electrode layer stacked;
[0093] The conductive substrate is a nickel plate with a thickness of 0.1 mm;
[0094] The fluid diffusion layer is a porous structure with a porosity of 90% and an average pore size of 2.5 mm; the raw materials for preparing the fluid diffusion layer include nickel powder, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the nickel powder, potassium carbonate and carboxymethyl cellulose is 95:3:2;
[0095] The catalytic electrode layer is a porous catalytic electrode with a porosity of 81%, an average pore size of 42 μm, and a specific surface area of 250 m 2 / g; the raw materials for preparing the catalytic electrode layer include Raney nickel alloy, potassium carbonate and carboxymethyl cellulose, and the mass ratio of the Raney nickel alloy, potassium carbonate and carboxymethyl cellulose is 95:3:2;
[0096] The thickness ratio of the fluid diffusion layer, the transport layer and the catalytic electrode layer is 4:1.
[0097] This embodiment also provides a method for preparing the above-mentioned integrated water electrolysis hydrogen production electrode, the preparation method comprising the following steps:
[0098] (1) nickel powder and potassium carbonate are mechanically mixed using a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during stirring and mixing is controlled to be 30° C. and the time is 120 min by using a double-layer slurry barrel and passing cooling water in the gap between the double layers to obtain a preparation slurry for a fluid diffusion layer; the mass ratio of nickel powder, potassium carbonate, carboxymethyl cellulose and water is 84.55:2.67:1.78:11;
[0099] The Raney nickel alloy and potassium carbonate are mechanically mixed by a powder mixer to obtain a mixed powder, and then carboxymethyl cellulose and water are mixed to prepare a binding solution, and then the mixed powder and the binding solution are stirred and mixed, and the temperature during the stirring and mixing is controlled to be 30° C. and the time is 120 minutes by using a double-layer slurry barrel and passing cooling water in the gap between the double layers to obtain a slurry for preparing a catalytic electrode layer; the mass ratio of the Raney nickel alloy, potassium carbonate, carboxymethyl cellulose and water is 84.55:2.67:1.78:11;
[0100] (2) coating the prepared slurry of the fluid diffusion layer on the surface to be coated of the conductive substrate, drying it in an oven to remove moisture, forming a fluid diffusion precursor layer, and obtaining a semi-finished electrode;
[0101] Among them, the drying temperature is 60℃ and the drying time is 9min;
[0102] (3) coating the surface of the fluid diffusion precursor layer with the slurry for preparing the catalytic electrode layer, drying it in an oven to remove moisture, the drying temperature is 60° C., the drying time is 9 min, to form a catalytic electrode precursor layer, and then sintering it at 1400° C. under the protection of a reducing atmosphere, the constant temperature time is 5 min, so that the conductive substrate, the fluid diffusion precursor layer and the catalytic electrode precursor layer are partially melted and integrated, and then placed in a KOH solution at a temperature of 60° C. for activation, to prepare the integrated water electrolysis hydrogen production electrode;
[0103] The gas in the reducing atmosphere includes nitrogen and hydrogen, and the volume fraction of hydrogen is 75%.
[0104] Example 4
[0105] The difference between this embodiment and embodiment 1 is that the average pore size of the fluid diffusion layer is 1 cm. At this time, the mass ratio of nickel powder, potassium carbonate, carboxymethyl cellulose and water in step (1) is 86.4:1.8:1.8:10, and the mass ratio of nickel powder, potassium carbonate and carboxymethyl cellulose in the integrated water electrolysis hydrogen production electrode is 96:2:2.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] Example 5
[0108] The difference between this embodiment and embodiment 1 is that the average pore size of the porous catalytic electrode is 150 μm. At this time, the mass ratio of nickel powder, potassium carbonate, carboxymethyl cellulose and water is 76.5:6.8:1.7:15, and the mass ratio of nickel powder, potassium carbonate and carboxymethyl cellulose in the integrated water electrolysis hydrogen production electrode is 90:8:2.
[0109] The rest of the preparation methods and parameters were the same as those in Example 1.
[0110] Example 6
[0111] The difference between this embodiment and embodiment 1 is that the thickness ratio of the fluid diffusion layer, the transport layer and the catalytic electrode layer is 2:1.5.
[0112] The rest of the preparation methods and parameters were the same as those in Example 1.
[0113] Example 7
[0114] The difference between this embodiment and embodiment 1 is that the thickness ratio of the fluid diffusion layer, the transport layer and the catalytic electrode layer is 6:0.3.
[0115] The rest of the preparation methods and parameters were the same as those in Example 1.
[0116] Example 8
[0117] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) is 1100°C.
[0118] The rest of the preparation methods and parameters were the same as those in Example 1.
[0119] Example 9
[0120] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) is 1500°C.
[0121] The rest of the preparation methods and parameters were the same as those in Example 1.
[0122] Example 10
[0123] The difference between this embodiment and embodiment 1 is that no sintering is performed in step (3).
[0124] The rest of the preparation methods and parameters were the same as those in Example 1.
[0125] Embodiment 11
[0126] The difference between this embodiment and embodiment 1 is that the activation temperature in step (3) is 10°C.
[0127] The rest of the preparation methods and parameters were the same as those in Example 1.
[0128] Example 12
[0129] The difference between this embodiment and embodiment 1 is that the activation temperature in step (3) is 90°C.
[0130] The rest of the preparation methods and parameters were the same as those in Example 1.
[0131] Example 13
[0132] The difference between this embodiment and embodiment 1 is that activation is not performed in step (3).
[0133] The rest of the preparation methods and parameters were the same as those in Example 1.
[0134] Comparative Example 1
[0135] The difference between this comparative example and Example 1 is that no fluid diffusion layer is provided, that is, step (2) is not performed.
[0136] The rest of the preparation methods and parameters were the same as those in Example 1.
[0137] Performance Testing
[0138] The integrated water electrolysis hydrogen production electrodes provided in the above embodiments and comparative examples were made into small chamber electrolytic cells, and their electrochemical performance was tested.
[0139] The specific steps of preparing the small chamber electrolytic cell include:
[0140] The integrated water electrolysis hydrogen production electrode is cut into a circle with a diameter of 60 mm;
[0141] Stack the anode end plate, electrode, diaphragm, sealing gasket, electrode, and cathode end plate in sequence to form an electrolysis chamber, and fasten them with bolts;
[0142] Connect the fastened chamber to the test bench, connect the alkali solution inlet channel, gas and liquid outlet channel, positive and negative poles of the power supply, etc., and prepare for testing.
[0143] The conditions for the electrochemical performance test are:
[0144] The test used 30% KOH solution, at a caustic temperature of 90°C, a circulation flow rate of 100mL / min, and first used 3000A / m 2 The electric density is tested for 48 hours, and then 2500A / m is used. 2 Electrical tightness test for 24 hours, record 2500A / m 2 Check the cell voltage under electrical density and the appearance of the electrode after the test.
[0145] The above test results are shown in Table 1.
[0146] Table 1
[0147]
[0148] analyze:
[0149] It can be seen from the above table that the electrolytic cell made based on the integrated water electrolysis hydrogen production electrode provided by the present invention can realize water electrolysis hydrogen production at a low voltage, enhance the catalytic capacity of the catalytic layer, and ensure that water electrolysis hydrogen production has lower energy consumption.
[0150] It can be seen from Examples 1 and 4-5 that if the average pore size of the fluid diffusion layer is too small, the fluid flow impedance will increase, resulting in a decrease in the fluid flow capacity, and a greater pressure will be required to drive the fluid flow. In severe cases, local eddy currents will occur, resulting in the liquid not being supplied to the electrode reaction zone in time, or the gas not being able to be discharged from the reaction zone in time, affecting the efficiency of the electrolysis reaction; if the average pore size of the porous catalytic electrode is too large, the catalyst specific surface area will be reduced and the catalyst conductive resistance will increase, which is reflected in the test results as a high chamber voltage and high electrolysis energy consumption.
[0151] It can be seen from Example 1 and Examples 6-7 that if the thickness ratio of the fluid diffusion layer, the transport layer, and the catalytic electrode layer is too small, the catalytic layer will be too thick or the transport layer will be too small, which will cause the gas-liquid transmission distance in the catalytic layer to be too long, the transmission resistance will increase, and it will be not conducive to the electrolysis reaction. The test results show that the electrolysis voltage is high; if the thickness ratio of the fluid diffusion layer, the transport layer, and the catalytic electrode layer is too large, the transport layer will be too large, which will increase the gas-liquid transmission distance and reduce the uniformity of fluid distribution. At the same time, due to the increase in distance, the electron transmission distance will increase, the resistance will increase, and the small chamber voltage will be higher.
[0152] It can be seen from Example 1 and Examples 8-9 that if the sintering temperature is too low, the metal powder bonding strength will be poor and powder will fall off during the electrolysis process; if the sintering temperature is too high, the metal will melt too much, forming large metal particles, reducing the reaction specific surface area, reducing the catalytic activity, and increasing the chamber voltage.
[0153] It can be seen from Example 1 and Example 10 that if sintering is not performed, it will be difficult to form the electrode, and the powder will fall off quickly during the electrolysis process, and the reaction cannot be sustained.
[0154] It can be seen from Example 1 and Examples 11-12 that if the activation temperature is too low, the Al in the catalyst will not be fully melted, and Al will continue to dissolve during the electrolysis test, contaminating the electrolyte, clogging the diaphragm, and increasing the chamber voltage; if the activation temperature is too high, it will cause excessive dissolution of Al in the alloy, reducing the catalytic ability, which is also manifested as a high chamber voltage.
[0155] It can be seen from Example 1 and Example 13 that if activation is not performed, a large amount of Al in the catalyst will melt in the electrolytic cell, polluting the electrolyte, seriously blocking the diaphragm, and causing a very high cell voltage.
[0156] It can be seen from Example 1 and Comparative Example 1 that if a fluid diffusion layer is not provided, the electrolytic reaction will lack electrolyte supply and gas diffusion channels, the electrode reaction capacity is extremely poor, and the cell voltage is very high.
[0157] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An integrated water electrolysis hydrogen production electrode, characterized in that: The integrated water electrolysis hydrogen production electrode comprises a conductive substrate, a fluid diffusion layer and a catalytic electrode layer which are stacked.
2. The integrated water electrolysis hydrogen production electrode according to claim 1, characterized in that: The conductive substrate comprises a nickel plate and / or a nickel-plated steel plate; And / or, the thickness of the conductive substrate is 0.05-0.1 mm.
3. The integrated water electrolysis hydrogen production electrode according to claim 1 or 2, characterized in that: The fluid transmitted by the fluid diffusion layer includes gas and liquid; And / or, the fluid diffusion layer is a porous structure; and / or, the porosity of the fluid diffusion layer is 70-98%; and / or, the average pore size of the fluid diffusion layer is 2-4 mm; And / or, the raw materials for preparing the fluid diffusion layer include metal powder, a first foaming agent and a first binder, and the mass ratio of the metal powder, the first foaming agent and the first binder is (80-95):(0.1-5):(0.5-5).
4. The integrated water electrolysis hydrogen production electrode according to any one of claims 1 to 3, characterized in that: The catalytic electrode layer is a porous catalytic electrode; and / or, the porosity of the porous catalytic electrode is 80-95%; And / or, the average pore size of the porous catalytic electrode is 5-100 μm; And / or, the specific surface area of the porous catalytic electrode is 80-300m 2 / g; And / or, the raw materials for preparing the catalytic electrode layer include an alloy material, a second foaming agent and a second binder, and the mass ratio of the alloy material, the second foaming agent and the second binder is (80-95):(0.1-5):(0.5-5); Preferably, the thickness ratio of the fluid diffusion layer, the transport layer and the catalytic electrode layer is (3-6):(0.5-1.5).
5. A method for preparing the integrated water electrolysis hydrogen production electrode according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Providing a conductive substrate, coating the surface of the conductive substrate to be coated with a slurry for preparing a fluid diffusion layer, and drying to form a fluid diffusion precursor layer to obtain a semi-finished electrode; The preparation slurry of the catalytic electrode layer is coated on the surface of the fluid diffusion precursor layer, and after drying, a catalytic electrode precursor layer is formed, which is then sintered and activated to obtain the integrated water electrolysis hydrogen production electrode.
6. The preparation method according to claim 5, characterized in that: The preparation slurry of the fluid diffusion layer includes metal powder, a first foaming agent, a first binder and water; And / or, the metal powder is nickel powder or nickel-based alloy powder; And / or, the slurry for preparing the catalytic electrode layer includes an alloy material, a second foaming agent, a second binder and water; And / or, the alloy material comprises a binary alloy, a ternary alloy or a multi-element alloy, and the metal species of the multi-element alloy are ≥ 4; And / or, the binary alloy includes any one of Raney nickel alloy, nickel-zinc alloy or nickel-iron alloy, or a combination of at least two thereof; and / or, the ternary alloy comprises a nickel-aluminum-molybdenum alloy; and / or, the multi-element alloy comprises a nickel-aluminum-zinc-molybdenum-iron-platinum alloy; and / or, the first blowing agent and the second blowing agent independently comprise carbonates; And / or, the first binder and the second binder independently include carboxymethyl cellulose and / or styrene-butadiene rubber.
7. The preparation method according to claim 5 or 6, characterized in that: The sintering process is carried out in a reducing atmosphere; and / or, the gas in the reducing atmosphere includes an inert gas and hydrogen; And / or, in the reducing atmosphere, the volume fraction of hydrogen is 60-80%; And / or, the sintering temperature is 1200-1400°C.
8. The preparation method according to claim 5 or 6, characterized in that: The specific steps of the activation include: placing the sintered product in an activation solution for activation; And / or, the activation solution includes KOH solution; And / or, the activation temperature is 50-80°C.
9. The preparation method according to claim 5 or 6, characterized in that: The preparation method comprises the following steps: (1) stirring and mixing metal powder, a first foaming agent, a first binder and water in a mass ratio of (80-95):(0.1-5):(0.5-5):(5-15) to obtain a slurry for preparing a fluid diffusion layer; The alloy material, the second foaming agent, the second binder and water are stirred and mixed in a mass ratio of (80-95):(0.1-5):(0.5-5):(5-15) to obtain a slurry for preparing a catalytic electrode layer; (2) coating the prepared slurry of the fluid diffusion layer on the surface to be coated of the conductive substrate, and forming a fluid diffusion precursor layer after drying to obtain a semi-finished electrode; Among them, the drying temperature is less than 120°C and the drying time is less than 10 minutes; (3) coating the surface of the fluid diffusion precursor layer with a slurry for preparing the catalytic electrode layer, drying it to form a catalytic electrode precursor layer, and then sintering it at 1200-1400°C under the protection of a reducing atmosphere, so that the conductive substrate, the fluid diffusion precursor layer and the catalytic electrode precursor layer are partially melted and integrated into one, and then placed in an activation solution with a temperature of 50-80°C for activation, thereby preparing the integrated water electrolysis hydrogen production electrode.