Preparation method of electrolytic copper foil with (111) texture

By using a titanium substrate with (0001) texture for electrodeposition, the problem of additive use in electrolytic copper foil preparation is solved, and the preparation of electrolytic copper foil with strong (111) texture and ultrafine grain size is achieved, reducing production Cost and improved performance, suitable for high energy density lithium batteries.

CN118979291AActive Publication Date: 2024-11-19HENAN UNIV OF SCI & TECH +1

Patent Information

Application Number
CN202411470646.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

The extensive use of additives in the existing electrolytic copper foil preparation methods leads to increased production costs and environmental risks, and it is difficult to effectively control the (111) texture of the copper foil.

Method used

Using a titanium substrate with (0001) texture as the cathode, an ultrafine crystalline electrolytic copper foil with (111) texture is formed in the electrolyte by electrodeposition, and the lattice matching degree of the copper foil is used for the atomic tight surface of titanium and the copper foil. Reduce the formation energy of copper crystal nuclei, promote the formation of (111) copper crystal nuclei and grain refinement, and avoid dependence on additives.

Benefits of technology

The strong (111) texture and ultrafine grain size of electrolytic copper foil are achieved, which reduces production costs, reduces the introduction of impurities, and has excellent comprehensive performance, which is suitable for the needs of high energy density and lightweight lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979291A_ABST
    Figure CN118979291A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrolytic copper foils, and particularly relates to a preparation method of an electrolytic copper foil with a (111) texture. The preparation method of the electrolytic copper foil with the (111) texture comprises the following steps that a titanium substrate with the (0001) texture serves as a cathode, electro-deposition is carried out in electrolyte to obtain the fine-grain electrolytic copper foil with the (111) texture, and the average grain size of the electrolytic copper foil is smaller than 0.2 micrometer. The stable adsorption active site density of Cu on the (0001) crystal face of titanium is relatively high, and the lattice matching degree of the (0001) atom close-packed face of titanium and the (111) atom close-packed crystal face of the copper foil is relatively high, so that the formation energy of (111) copper crystal nucleuses can be reduced, the formation of the (111) copper crystal nucleuses can be promoted, further, the texture formation and grain refinement of the copper foil (111) are promoted, and the ultra-fine grain electrolytic copper foil with a strong (111) texture is obtained; and the comprehensive performance of the electrolytic copper foil is synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic copper foil, and in particular to a method for preparing an electrolytic copper foil with a (111) texture. Background Art

[0002] Electrolytic copper foil is a key basic material for lithium battery current collectors, printed circuit boards and packaging substrates, and is widely used in chip packaging, printed circuits and new energy fields. In lithium batteries, electrolytic copper foil is the carrier of negative electrode active materials, acting as an electron collector and conductor, and determines the battery energy density. In printed circuit boards and packaging substrates, electrolytic copper foil plays the role of interconnection, insulation and support, and determines the signal transmission speed, energy loss and characteristic impedance.

[0003] In industrial production, under the action of the electric field, the copper ions in the copper sulfate electrolyte are reduced and precipitated on the surface of the titanium cathode roller to form metallic copper. At the same time, the titanium cathode roller rotates continuously at a uniform speed, and the copper ions are continuously electrodeposited onto the cathode titanium surface. When the deposition reaches a certain thickness, it is peeled off and rolled to form an electrolytic copper foil. In principle, the electrolytic copper foil is the electrochemical continuous crystallization product of copper ions on the cathode titanium. During the electrocrystallization process, after the reduced newly adsorbed copper atoms reach the cathode titanium surface, they nucleate and grow along the original crystal structure of the titanium substrate, gradually forming an initial deposition layer.

[0004] The microstructure of the cathode titanium surface directly affects the nucleation and growth of copper ions, and thus affects the microstructure of the electrolytic copper foil. As integrated circuits gradually become denser, multi-layered, and thinner, lithium batteries are also developing in the direction of high energy density and light weight, which requires copper foil to be thinner and thinner. At this time, the initial deposition layer of the ultra-thin copper foil is crucial to the entire electrolytic copper foil.

[0005] Grain refinement of electrolytic copper foil can make it have high tensile strength and high elongation at the same time. In addition, a large number of studies have shown that (111) texture not only makes electrolytic copper foil have good mechanical properties (tensile strength and elongation), but also facilitates the uniform deposition and nucleation of lithium during the charging and discharging process of lithium batteries, thereby improving the service life of lithium batteries. At present, most reports on grain refinement and texture control of electrolytic copper foil focus on additive control.

[0006] The Chinese patent application with application publication number CN118028918A and application publication date May 14, 2024 discloses a copper foil composite additive and a method for preparing a highly oriented electrolytic copper foil. The composite additive includes additive A as a brightener, additive B as a wetting agent and additive C as a leveling agent. Additive A is at least one of sulfonated thiacalix[4]arene, sulfonated thiacalix[6]arene and sulfonated thiacalix[8]arene. The rigid structure of sulfonated thiacalixarene is used to make the calixarene adsorbed on the cathode form a directional arrangement with the sulfonic acid group upward. Copper ions can only approach the cathode from the edge of the calixarene, resulting in the directional growth of copper grains, which is beneficial to the precipitation of copper (111) crystal plane, thereby improving the tensile strength of the copper foil.

[0007] However, in industrial production, a large amount of additives will not only increase the production cost of electrolytic copper foil, but may also introduce impurity elements into the copper foil. In addition, a large amount of additives has certain hidden dangers to the environment. Summary of the invention

[0008] The object of the present invention is to provide a method for preparing an electrolytic copper foil having a (111) texture, so as to solve the problem of using a large amount of additives when preparing an electrolytic copper foil having a (111) texture.

[0009] In order to solve the above technical problems, the technical solution of the method for preparing an electrolytic copper foil with a (111) texture of the present invention is as follows: A method for preparing an electrolytic copper foil with a (111) texture comprises the following steps: using a titanium substrate with a (0001) texture as a cathode, and performing electrodeposition in an electrolyte to obtain a fine-grained electrolytic copper foil with a (111) texture, wherein the average grain size of the electrolytic copper foil is less than 0.2 μm.

[0010] The present invention provides a method for preparing an electrolytic copper foil with a (111) texture in a pioneering manner. A titanium substrate with a (0001) texture is used as a cathode. Since the (0001) crystal plane of titanium is an atomic close-packed plane, the density of stable adsorption active sites of Cu on its surface is higher. Moreover, the lattice matching degree between the (0001) crystal plane of titanium and the (111) atomic close-packed crystal plane of copper foil is higher, which can reduce the formation energy of (111) copper nuclei, facilitate the formation of (111) copper nuclei, and make copper ions uniformly and densely nucleate on the surface of the cathode titanium substrate, thereby promoting the formation of the (111) texture of the copper foil and grain refinement, thereby obtaining an ultrafine-grained electrolytic copper foil with a strong (111) texture, and realizing the synergistic improvement of the comprehensive performance of the electrolytic copper foil.

[0011] In order to further improve the (0001) texture performance of the titanium substrate, preferably, the method for preparing the titanium substrate comprises the following steps: hot rolling the forged pure titanium at 400-450° C., and then cold rolling and annealing.

[0012] In order to further improve the (0001) texture performance of the titanium substrate, preferably, the deformation amount during hot rolling is 60-70%.

[0013] In order to further improve the (0001) texture performance of the titanium substrate, preferably, the total deformation during the cold rolling is 50-60%.

[0014] In order to further improve the (0001) texture properties of the titanium substrate, preferably, multiple cold rolling passes are used during cold rolling, and the deformation amount of each cold rolling pass is 10-15%.

[0015] In order to further refine the grains, preferably, the annealing temperature is 500-550° C. and the annealing time is 1-2 hours. Static recrystallization during the annealing process can refine the titanium grains, and the titanium finally obtained has fine equiaxed crystals with a grain size of 8-13.

[0016] In order to further improve the deposition quality during electrodeposition and refine the copper foil grains, preferably, the electrolyte includes 100-120 g / L of CuSO4, 105-120 g / L of H2SO4 and 40-50 mg / L of HCl.

[0017] In order to further improve the deposition efficiency of electrodeposition, preferably, the electrodeposition temperature is 40-60°C and the current density is 30-50A / dm 2 .

[0018] In order to further obtain an extremely thin ultrafine-grained electrolytic copper foil, preferably, the thickness of the prepared electrolytic copper foil is 4.5-6 μm, and the average grain size is 0.15-0.17 μm.

[0019] The beneficial effects of the present invention are as follows: the electrolytic copper foil prepared by the preparation method of the present invention has a strong (111) texture, and the average grain size is less than 0.2 μm, which is more than 50% smaller than the grain size of conventional copper foil at present, thereby obtaining an ultrafine-grained electrolytic copper foil with (111) texture and excellent comprehensive performance. In addition, the preparation method of the present invention does not require the addition of multiple complex additives, greatly reduces the production cost, is conducive to green environmental protection, and provides a new preparation method for electrolytic copper foil with comprehensive excellence. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is an orientation imaging diagram of the titanium substrate of Example 1 of the present invention; Figure 2 is the inverse pole figure of the titanium substrate of Example 1 of the present invention; Figure 3 This is a grain size distribution diagram of the titanium substrate of Example 1 of the present invention; Figure 4This is an orientation imaging diagram of the electrolytic copper foil prepared in Example 1 of the present invention; Figure 5 This is a grain size distribution diagram of the electrolytic copper foil prepared in Example 1 of the present invention; Figure 6 The reverse pole figure of the electrolytic copper foil prepared in Example 1 of the present invention; Figure 7 This is a stress-strain curve diagram of the electrolytic copper foil prepared in Example 1 of the present invention; Figure 8 This is an orientation imaging diagram of the electrolytic copper foil prepared in Example 2 of the present invention; Fig. 9 This is a grain size distribution diagram of the electrolytic copper foil prepared in Example 2 of the present invention; Fig.10 The reverse pole figure of the electrolytic copper foil prepared in Example 2 of the present invention; Fig.11 is a stress-strain curve diagram of the electrolytic copper foil prepared in Example 2 of the present invention; Fig.12 This is an orientation imaging diagram of the electrolytic copper foil prepared in Comparative Example 1 of the present invention; Fig.13 This is a grain size distribution diagram of the electrolytic copper foil prepared in Comparative Example 1 of the present invention; Fig.14 The reverse pole figure of the electrolytic copper foil prepared in Comparative Example 1 of the present invention; Fig.15 This is a stress-strain curve of the electrolytic copper foil prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The technical concept of the method for preparing the electrolytic copper foil with (111) texture of the present invention is as follows: The prior art effectively promotes the highly oriented growth of the (111) surface of copper foil by regulating additives, thereby achieving the production of high tensile strength copper foil. The present invention innovatively utilizes the higher Cu adsorption active sites on the atomic close-packed surface of the substrate during electrodeposition and the degree of matching between the Cu adsorption active sites and the close-packed surface lattice of the copper foil, and regulates the preferred orientation of the substrate grains to reduce the formation energy of the (111) copper nuclei, thereby promoting the formation of the (111) texture of the copper foil and grain refinement, and achieving a strong (111) texture of the ultrafine-grained electrolytic copper foil.

[0022] It can be understood that the electrolyte used in the present invention is prepared from analytically pure copper sulfate pentahydrate, sulfuric acid and water, and the mass concentration of CuSO4 in the electrolyte is based on commercially available analytically pure copper sulfate pentahydrate. Similarly, the mass concentration of H2SO4 is based on commercially available concentrated sulfuric acid (mass fraction 98%), and the mass concentration of HCl is based on commercially available hydrochloric acid (mass fraction 37%).

[0023] The present invention is described in detail below in conjunction with specific examples. The raw materials used in the following examples are all conventional commercial products and are well known to those skilled in the art.

[0024] 1. Specific embodiment of the method for preparing the electrolytic copper foil with (111) texture of the present invention Example 1 The method for preparing the electrolytic copper foil with (111) texture in this embodiment is as follows: (1) Preparation of titanium substrate: First, cast pure titanium was prepared by cold crucible vacuum suspension melting, and then free forging was performed at a temperature of 950°C to obtain forged pure titanium. The forged pure titanium was hot rolled at a temperature of 450°C and a hot rolling deformation of 70%. Then, the pure titanium was cold rolled with a total cold rolling deformation of 50%. Five cold rolling passes were used, with a deformation of 10% per pass. Then, annealing was performed at a temperature of 500°C and an annealing time of 1 h to obtain a pure titanium plate with a (0001) texture. Before electrodeposition, mechanical polishing and electrolytic polishing were performed to remove the oxide layer to obtain a smooth surface for use as a cathode.

[0025] It can be understood that in practical industrial applications, pure titanium with a (0001) texture can be made into a cathode roller titanium cylinder. During electrodeposition, the cathode roller rotates continuously at a uniform speed, and copper ions are continuously electrodeposited onto the cathode titanium surface. When the deposition reaches a certain thickness, the foil is peeled off and rolled up to form an extremely thin fine-grained electrolytic copper foil. The preparation method of the cathode roller titanium cylinder can refer to the existing technology. For example, the pure titanium plate with a (0001) texture can be rolled and welded to form a cathode roller titanium cylinder.

[0026] Electron backscatter diffractometer (EBSD, Bruker QUANTAX CrystAlign 400i) was used to detect and collect microstructural information such as grain size, grain orientation, and local orientation difference on the surface of pure titanium. The orientation imaging map, inverse pole figure, and grain size distribution map of the prepared pure titanium with (0001) texture are shown in Figure 2. Figure 1 , Figure 2 and Figure 3 As shown. Figure 1-2 It can be seen that the microstructure of pure titanium is composed of fine equiaxed crystals, among which there are a large number of red grains with (0001) crystal plane orientation, and the pure titanium substrate has obvious (0001) texture. Using the TSL OIM Analysis software in the electron backscatter diffractometer (EBSD, BrukerQUANTAX CrystAlign 400i), the grain size on the sample surface was statistically analyzed by the intercept method to obtain the grain size distribution diagram of the pure titanium surface ( Figure 3), and calculated the average value thereof, to obtain an average grain size of the pure titanium substrate of 3.98 μm, and the grain size of grains of this size reached level 13; in other embodiments, the grain size (measured in terms of average grain size) of the prepared titanium substrate is in the range of levels 8 to 13.

[0027] (2) Electrodeposition: Add copper sulfate pentahydrate, sulfuric acid and hydrochloric acid to deionized water to prepare an electrolyte, wherein the mass concentration of CuSO4 in the electrolyte is 100 g / L, the mass concentration of H2SO4 is 105 g / L, and the mass concentration of HCl is 40 mg / L; add the electrolyte to an electrolytic cell, use the pure titanium with (0001) texture prepared in step (1) as the cathode, use iridium-plated titanium as the anode, and perform direct current electrodeposition under stirring conditions. The electrodeposition temperature is 60°C and the current density is 30 A / dm 2 , an electrolytic copper foil with a thickness of 6 μm was obtained.

[0028] Electron backscatter diffractometer was used to detect and collect information on the microstructure of the copper foil surface, such as grain size, grain orientation, and local orientation difference. The electrolytic copper foil has a strong (111) texture and fine equiaxed grains. The orientation imaging map, grain size distribution map, and anti-pole figure of the electrolytic copper foil are shown in Figure 1. Figure 4 , 5 and shown in 6. Depend on Figure 4 It can be found that the microstructure of the copper foil is composed of fine equiaxed grains, among which there are a large number of blue grains with (111) crystal plane orientation. Figure 5 From the grain size distribution diagram of the copper foil, it can be statistically determined that the average grain size of the copper foil is 0.15 μm. Figure 6 The inverse pole figure shows that the copper foil has an obvious (111) texture. The mechanical properties of the copper foil were tested, and the stress-strain curves obtained were as follows: Figure 7 As shown, from Figure 7 It can be seen that the tensile strength of the copper foil is 426.5MPa, and the elongation obtained by the test is 5.1%.

[0029] Example 2 The preparation method of the electrolytic copper foil with (111) texture in this embodiment is basically the same as that in Example 1, except that the electrodeposition process parameters are changed, specifically: (2) Electrodeposition: add copper sulfate pentahydrate, sulfuric acid and hydrochloric acid to deionized water to prepare an electrolyte, wherein the mass concentration of CuSO4 in the electrolyte is 120 g / L, the mass concentration of H2SO4 is 120 g / L, and the mass concentration of HCl is 50 mg / L; add the electrolyte to an electrolytic cell, use the pure titanium with (0001) texture prepared in step (1) as the cathode, use iridium-plated titanium as the anode, and perform direct current electrodeposition under stirring conditions, the electrodeposition temperature is 40°C, and the current density is 50 A / dm 2, an electrolytic copper foil with a thickness of 4.5 μm was obtained.

[0030] The electrolytic copper foil has fine equiaxed grains and a strong (111) texture. The orientation imaging diagram, grain size distribution diagram and inverse pole figure of the electrolytic copper foil are shown in Figs. Figure 8 , 9 and shown in 10. Depend on Figure 8 It can be found that the microstructure of the copper foil is composed of fine equiaxed grains, among which there are a large number of blue grains with (111) crystal planes. Fig. 9 From the grain size distribution diagram of the copper foil, it can be statistically determined that the average grain size of the copper foil is 0.17 μm. Fig.10 From the inverse pole figure, it can be found that the copper foil has an obvious (111) texture. The stress-strain curve obtained by the test is shown in Fig.11 As shown, the tensile strength of the copper foil is 434.1 MPa, and the elongation obtained by the test is 4.6%.

[0031] 2. Comparison Comparative Example 1 The method for preparing the electrolytic copper foil with (111) texture in this comparative example is basically the same as that in Example 1, except that the crystal surface texture of the titanium substrate is changed, specifically: (2) Pure titanium with crystal surface texture was used as cathode and iridium-plated titanium was used as anode. Direct current electrodeposition was carried out under stirring conditions to obtain electrolytic copper foil with a thickness of 0.6 μm.

[0032] The orientation imaging diagram, grain size distribution diagram and inverse pole figure of the electrolytic copper foil obtained are shown as follows: Fig.12 , 13 and shown in 14. Depend on Fig.12 It can be found that the copper foil is composed of relatively coarse block and flake grains, and the microstructure is uneven. Fig.13 From the grain size distribution diagram of the copper foil, it can be statistically obtained that the average grain size of the copper foil is 0.52 μm, which is more than three times that of the electrolytic copper foil in Example 1. Fig.14 From the inverse pole figure, it can be found that the texture of the copper foil is not a single (111) texture, but there are two textures (111) and (110). The stress-strain curve obtained by the test is as follows Fig.15 As shown, the tensile strength of the copper foil is 286.9 MPa, and the elongation obtained by the test is 3.5%.

[0033] The specific structural characteristic parameters and performance indicators of the electrolytic copper foils prepared in various embodiments and comparative examples are shown in Table 1.

[0034] Table 1 Specific structural characteristic parameters and mechanical properties of electrolytic copper foil Serial number Grain size / μm (111) Texture strength Tensile strength / MPa Elongation Example 1 0.15 1.675 426.5 5.1% Example 2 0.17 1.520 434.1 4.6% Comparative Example 1 0.52 1.112 286.9 3.5% The above is only a preferred specific implementation of the present invention; however, the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solution and its improved conception within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an electrolytic copper foil having a (111) texture, It is characterized in that The following steps are involved: A titanium substrate with a (0001) texture is used as a cathode, and electrodeposition is performed in an electrolyte to obtain a fine-grained electrolytic copper foil with a (111) texture, wherein the average grain size of the electrolytic copper foil is less than 0.2 μm.

2. The method for preparing an electrolytic copper foil having a (111) texture according to claim 1, It is characterized in that The preparation method of the titanium substrate comprises the following steps: hot rolling the forged pure titanium at 400-450° C., and then cold rolling and annealing.

3. The method for preparing an electrolytic copper foil having a (111) texture according to claim 2, It is characterized in that The deformation during hot rolling is 60-70%.

4. The method for preparing an electrolytic copper foil having a (111) texture according to claim 2, It is characterized in that The total deformation during the cold rolling is 50-60%.

5. The method for preparing an electrolytic copper foil having a (111) texture according to claim 2 or 4, It is characterized in that Multiple cold rolling passes are used during cold rolling, and the deformation of each cold rolling pass is 10~15%.

6. The method for preparing an electrolytic copper foil having a (111) texture according to claim 2, It is characterized in that The annealing temperature is 500-550° C., and the annealing time is 1-2 hours.

7. The method for preparing an electrolytic copper foil having a (111) texture according to claim 1, It is characterized in that The electrolyte includes 100-120 g / L of CuSO 4 , 105~120g / L H 2 SO 4 and 40~50 mg / L HCl.

8. The method for preparing an electrolytic copper foil having a (111) texture according to claim 1, It is characterized in that The electrodeposition temperature is 40-60°C and the current density is 30-50A / dm 2 .

9. The method for preparing an electrolytic copper foil having a (111) texture according to claim 1, It is characterized in that The thickness of the prepared electrolytic copper foil is 4.5~6 μm, and the average grain size is 0.15~0.17 μm.

Citation Information

Patent Citations

  • Titanium sheet and copper foil production drum

    CN113260727A

  • Method for preparing low-warpage ultrathin electrolytic copper foil through reduction process

    CN113481550A

  • Nano twin-crystal copper foil and preparation method thereof

    CN113621998A

  • Room-temperature electro-deposition preparation method of copper foil with high crystal face preferred orientation

    CN113802155A

  • Composite thermomechanical treatment process for refining titanium material grains

    CN115717225A

Cited By

  • Heat-resistant copper foil and preparation method thereof

    CN120776403A

  • Method for quantitatively controlling grain size of electro-deposition copper foil through power ultrasound

    CN120866892A

  • Preparation method of high-precision automobile connector red copper belt

    CN121222858A