High-flame-retardant polypropylene fiber and preparation method thereof

By combining polypropylene fiber slices with flame retardant masterbatches, high flame retardant polypropylene fibers are prepared, which solves the problem of insufficient flame retardant in the prior art, and achieves the high flame retardant performance and wider application of polypropylene fibers.

CN118979312AInactive Publication Date: 2024-11-19HUAIAN YONGCHENG NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410939814.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing high-strength flame-retardant polypropylene hollow fibers have insufficient flame retardant properties, resulting in a short service life and limited application range.

Method used

The combination of polypropylene fiber-forming slices and flame retardant masterbatches, including decabromide diphenyl ether, antimony trioxide and flame retardant, is prepared by preheating, stirring, drying, vacuum twin screw extrusion and spinning molding. High flame retardant polypropylene fiber improves its flame retardant performance.

Benefits of technology

It significantly improves the flame retardant properties of polypropylene fiber, extends service life and expands its scope of application, making it available for use in a variety of industrial fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979312A_ABST
    Figure CN118979312A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical fibers, and provides a high-flame-retardant polypropylene fiber and a preparation method thereof. The polypropylene fiber is prepared from the following raw materials in parts by weight: 40 to 65 parts of polypropylene fiber forming slices and 35 to 60 parts of flame-retardant master batch; wherein the flame-retardant master batch is a mixture of 20-40 parts of decabromodiphenyl ether, 30-70 parts of antimony trioxide, 10-15 parts of a flame retardant, 1-8 parts of an antioxidant and 1-15 parts of a coupling agent; the coupling agent is a mixture of poly (2-hydroxyethyl terephthalate) resin and dioctyl pyrophosphate acyloxy, and the mass ratio of the poly (2-hydroxyethyl terephthalate) resin to the dioctyl pyrophosphate acyloxy is 1: (2-5). The high-flame-retardant polypropylene fiber contains decabromodiphenyl ether and antimony trioxide, an organic flame retardant and an inorganic flame retardant are combined, and meanwhile, the flame retardant is added, so that the flame retardance of the polypropylene fiber can be greatly improved, and the polypropylene fiber has high flame retardance; the service life of a polypropylene fiber product can be further prolonged, the application range of the polypropylene fiber product is expanded, and the polypropylene fiber product can be used in various industrial fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical fibers, and in particular relates to a highly flame-retardant polypropylene fiber and a preparation method thereof. Background Art

[0002] Polypropylene fiber is a synthetic fiber spun from isotactic polypropylene obtained by polymerization of propylene; polypropylene fiber is divided into long fiber, short fiber, etc.

[0003] Early propylene polymerization could only produce paper products with low polymerization degree, which belonged to non-crystalline compounds and had no practical value. In 1954, Ziegler and Natta invented the Ziegler-Natta catalyst and produced crystalline polypropylene with high stereoregularity, which was called isotactic polypropylene or isotactic polypropylene. This research result opened up a new direction in the field of polymerization and laid the foundation for the large-scale industrial production of polypropylene and its wide application in plastic products and fiber production. After 1980, with the development of new technologies for polypropylene and manufacturing polypropylene fibers, especially the invention of metallocene catalysts, the quality of polypropylene resin has been significantly improved. Due to the improvement of its stereoregularity (isotacticity can reach 99.5%), the intrinsic quality of polypropylene fibers has been greatly improved. In the mid-1980s, polypropylene fine fibers replaced part of cotton fibers and were used in textile fabrics and non-woven fabrics. With the development of one-step BCF spinning machines, air texturing machines and composite spinning machines, as well as the emergence and rapid development of non-woven fabrics, the use of polypropylene fibers in decoration and industrial use has been further broadened. In addition, countries around the world are also quite active in the research and development of polypropylene fibers. The popularization and improvement of differentiated fiber production technology has greatly expanded the application areas of polypropylene fibers. The above content is information that can be found on Baidu Encyclopedia.

[0004] In the related prior art, for example, a Chinese invention patent application discloses a high-strength flame-retardant polypropylene hollow fiber and a manufacturing method thereof, with a publication number of CN110331462A. The specific technical solution disclosed in the patent is: "The high-strength flame-retardant polypropylene hollow fiber is composed of the following components in parts by weight: 80-120 parts of high molecular weight polypropylene, 8-12 parts of ultra-high molecular weight polyethylene, 0.08-0.15 parts of antioxidant, 10-20 parts of halogen-free flame retardant, and 3-8 parts of carbon fiber." The aforementioned high-strength flame-retardant polypropylene hollow fiber is prepared by using high molecular weight polypropylene, ultra-high molecular weight polyethylene and other ingredients to have high strength and flame retardant properties; however, in actual use, its flame retardancy is still not ideal, resulting in a short service life of the polypropylene fiber and a limited scope of application. Summary of the invention

[0005] In view of the above-mentioned problems existing in the prior art, the object of the present invention is to provide a highly flame-retardant polypropylene fiber and a preparation method thereof, which can greatly improve the flame retardancy of the polypropylene fiber and make it have the characteristics of high flame retardancy.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A highly flame-retardant polypropylene fiber, the polypropylene fiber is composed of the following raw materials in parts by weight: 40-65 parts of polypropylene fiber chips and 35-60 parts of flame-retardant masterbatch; wherein the flame-retardant masterbatch is a mixture of 20-40 parts of decabromodiphenyl ether, 30-70 parts of antimony trioxide, 10-15 parts of flame retardant, 1-8 parts of antioxidant and 1-15 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate bis(hydroxyethyl) resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate bis(hydroxyethyl) resin to dioctyl pyrophosphate acyloxy is 1:(2-5).

[0008] As a preferred technical solution of the present invention, the polypropylene fiber chips are 57 parts and the flame retardant masterbatch is 43 parts; wherein the flame retardant masterbatch is a mixture of 24 parts of decabromodiphenyl ether, 46 parts of antimony trioxide, 13 parts of flame retardant, 2 parts of antioxidant and 15 parts of coupling agent.

[0009] As a preferred technical solution of the present invention, the antioxidant is antioxidant 1010.

[0010] As a preferred technical solution of the present invention, the mass ratio of the polyethylene terephthalate resin to dioctyl pyrophosphate is 1:2.5.

[0011] The present invention also provides a method for preparing a highly flame-retardant polypropylene fiber as described above, the method comprising the following steps:

[0012] S1, prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 90-105°C for preheating, and use a stirrer to continuously stir for 0.5-1h, cool at a temperature of 120-140°C, use a dryer for drying for 5-8h, and obtain a mixture;

[0013] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0014] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0015] As a preferred technical solution of the present invention, the filter has a mesh size of 120-175.

[0016] As a preferred technical solution of the present invention, the preheating temperature in step S1 is set to 100°C, wherein the stirring time t1 is 2.5h; the drying temperature in the drying machine is adjusted to 120°C, and the drying time t2 is 6h.

[0017] The invention relates to a highly flame-retardant polypropylene fiber and a preparation method thereof, which have the following beneficial effects: the highly flame-retardant polypropylene fiber of the invention contains decabromodiphenyl ether and antimony trioxide, combines an organic flame retardant with an inorganic flame retardant, and adds a flame retardant, on this basis, can greatly improve the flame retardancy of the polypropylene fiber, so that it has high flame retardant performance; can further prolong the service life of polypropylene fiber products and expand their scope of application, and can be used in a variety of industrial fabrics.

[0018] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is an actual product diagram of polypropylene fiber in the prior art;

[0020] Figure 2 This is a picture of an actual product of highly flame-retardant polypropylene fiber obtained through the application of the present invention;

[0021] Figure 3 The present invention provides a flow chart of the method for preparing highly flame-retardant polypropylene fiber. DETAILED DESCRIPTION

[0022] The embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0023] Common polypropylene fibers in the prior art are Figure 1 , and the high flame retardant polypropylene fiber prepared by the method of the present invention is Figure 2 The present invention provides 12 examples and 5 comparative examples, wherein the preparation process used in Examples 1-12 is shown in Figure 3 shown.

[0024] Preparation of raw materials

[0025] Polypropylene fiber chips and flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of decabromodiphenyl ether, antimony trioxide, flame retardant, antioxidant and coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate.

[0026] Example 1

[0027] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0028] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 40 parts of polypropylene fiber chips and 60 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 20 parts of decabromodiphenyl ether, 50 parts of antimony trioxide, 10 parts of flame retardant, 8 parts of antioxidant, and 12 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 90°C for preheating, and use a stirrer to continuously stir for a time t1 of 0.8h (0.5-1h), cool at a temperature of 120°C, use a dryer for a drying time t2 of 5h (5-8h), and obtain a mixture;

[0029] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0030] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0031] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0032] Example 2

[0033] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0034] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 42 parts of polypropylene fiber chips and 58 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 22 parts of decabromodiphenyl ether, 48 parts of antimony trioxide, 12 parts of flame retardant, 8 parts of antioxidant, and 10 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2.3; preheat the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 90°C, and use a stirrer to continuously stir for a time t1 of 0.8h (0.5-1h), cool at a temperature of 120°C, and use a dryer for a drying time t2 of 5h (5-8h) to obtain a mixture;

[0035] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0036] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0037] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0038] Example 3

[0039] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0040] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 45 parts of polypropylene fiber chips and 55 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 25 parts of decabromodiphenyl ether, 45 parts of antimony trioxide, 13 parts of flame retardant, 7 parts of antioxidant, and 10 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2.5; preheat the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 101°C, and use a stirrer to continuously stir for a time t1 of 0.6h (0.5-1h), cool at a temperature of 125°C, and use a dryer for a drying time t2 of 7.5h (5-8h), to obtain a mixture;

[0041] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0042] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0043] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0044] Example 4

[0045] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0046] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 51 parts of polypropylene fiber chips and 49 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 30 parts of decabromodiphenyl ether, 45 parts of antimony trioxide, 15 parts of flame retardant, 2 parts of antioxidant, and 8 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2.6; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 101°C for preheating, and use a stirrer to continuously stir for a time t1 of 0.6h (0.5-1h), cool at a temperature of 125°C, use a dryer for a drying time t2 of 7.5h (5-8h), and obtain a mixture;

[0047] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0048] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0049] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0050] Example 5

[0051] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0052] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 55 parts of polypropylene fiber chips and 45 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 32 parts of decabromodiphenyl ether, 38 parts of antimony trioxide, 10 parts of flame retardant, 7 parts of antioxidant, and 13 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:3; preheat the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 101°C, and use a stirrer to continuously stir for a time t1 of 0.6h (0.5-1h), cool at a temperature of 125°C, and use a dryer for a drying time t2 of 7.5h (5-8h), to obtain a mixture;

[0053] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0054] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0055] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0056] Example 6

[0057] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0058] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 60 parts of polypropylene fiber chips and 40 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 40 parts of decabromodiphenyl ether, 30 parts of antimony trioxide, 12 parts of flame retardant, 5 parts of antioxidant, and 13 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:3.12; preheat the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 100°C, and use a stirrer to continuously stir for a time t1 of 0.8h (0.5-1h), cool at a temperature of 135°C, and use a dryer for a drying time t2 of 5h (5-8h), to obtain a mixture;

[0059] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0060] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0061] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0062] Example 7

[0063] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0064] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 63 parts of polypropylene fiber chips and 47 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 20 parts of decabromodiphenyl ether, 50 parts of antimony trioxide, 10 parts of flame retardant, 8 parts of antioxidant, and 12 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 100°C for preheating, and use a stirrer to continuously stir for a time t1 of 0.8h (0.5-1h), cool at a temperature of 135°C, use a dryer for a drying time t2 of 5h (5-8h), and obtain a mixture;

[0065] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0066] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0067] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0068] Example 8

[0069] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0070] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 62 parts of polypropylene fiber chips and 48 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 20 parts of decabromodiphenyl ether, 50 parts of antimony trioxide, 10 parts of flame retardant, 8 parts of antioxidant, and 12 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2.7; preheat the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 100°C, and use a stirrer to continuously stir for a time t1 of 0.7h (0.5-1h), cool at a temperature of 125°C, and use a dryer for a drying time t2 of 7h (5-8h) to obtain a mixture;

[0071] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0072] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0073] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0074] Example 9

[0075] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0076] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 57 parts of polypropylene fiber chips and 43 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 24 parts of decabromodiphenyl ether, 46 parts of antimony trioxide, 13 parts of flame retardant, 2 parts of antioxidant, and 15 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:2.5; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 100°C for preheating, and use a stirrer to continuously stir for 2.5h (0.5-1h), cool at 120°C, use a dryer for drying for 6h (5-8h), and obtain a mixture;

[0077] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0078] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0079] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0080] Example 10

[0081] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0082] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 49 parts of polypropylene fiber chips and 51 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 25 parts of decabromodiphenyl ether, 45 parts of antimony trioxide, 13 parts of flame retardant, 2 parts of antioxidant, and 15 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:4; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 90°C for preheating, and use a stirrer to continuously stir for a time t1 of 0.8h (0.5-1h), cool at a temperature of 120°C, use a dryer for a drying time t2 of 5h (5-8h), and obtain a mixture;

[0083] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0084] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0085] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0086] Embodiment 11

[0087] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0088] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 64 parts of polypropylene fiber chips and 46 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 36 parts of decabromodiphenyl ether, 34 parts of antimony trioxide, 13 parts of flame retardant, 2 parts of antioxidant, and 15 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:4.9; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 102°C for preheating, and use a stirrer to continuously stir for 1h (0.5-1h), cool at a temperature of 135°C, use a dryer for drying for 6h (5-8h), and obtain a mixture;

[0089] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0090] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0091] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0092] Example 12

[0093] A highly flame-retardant polypropylene fiber, a method for preparing the highly flame-retardant polypropylene fiber comprises the following steps

[0094] S1. Prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, wherein the ratio is 65 parts of polypropylene fiber chips and 45 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 20 parts of decabromodiphenyl ether, 58 parts of antimony trioxide, 10 parts of flame retardant, 2 parts of antioxidant, and 10 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate resin to dioctyl pyrophosphate acyloxy is 1:5; place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 105°C for preheating, and use a stirrer to continuously stir for 1h (0.5-1h), cool at a temperature of 140°C, use a dryer for drying for 8h (5-8h), and obtain a mixture;

[0095] S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed;

[0096] S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

[0097] The filter mesh number is 130 mesh (120-175 mesh is suitable), the temperatures of the three zones of the screw are: Zone 1: 90°C; Zone 2: 100°C; Zone 3: 105°C. Pre-spinning oiling: 2.1%; original yarn oiling wet rate: 12% and other technical parameters.

[0098] It should be noted that the vacuum twin-screw extruder used in the present invention can be a twin-screw extruder of model SAT65 produced by Jiangsu Yuesheng Technology Co., Ltd.

[0099] Comparative Example 1

[0100] The difference from Example 1 is that in the preparation of the highly flame-retardant polypropylene fiber of the present invention, no flame-retardant masterbatch is added.

[0101] Comparative Example 2

[0102] The difference from Example 1 is that no decabromodiphenyl ether raw material is added to the flame retardant masterbatch preparation components of the present invention.

[0103] Comparative Example 3

[0104] The difference from Example 1 is that no antimony trioxide raw material is added to the flame retardant masterbatch preparation components of the present invention.

[0105] Comparative Example 4

[0106] The difference from Example 1 is that no flame retardant raw materials are added to the preparation components of the flame retardant masterbatch applied in the present invention.

[0107] Comparative Example 5

[0108] The difference from Example 1 is that the raw materials of decabromodiphenyl ether and antimony trioxide are no longer added to the flame retardant masterbatch preparation components of the present invention.

[0109] The performance test of the embodiments 1-12 and comparative examples 1-5 of the present invention was carried out, and the test items included mechanical property test and flame retardant property test; the test method of the mechanical property test was to take out three flame retardant polypropylene staple fiber samples from the embodiments 1-12 and comparative examples 1-5 respectively, and then carry out elongation at break test on the above samples with reference to GB / T14337-1993 "Test method for breaking strength and elongation at break of synthetic staple fibers", and take the average value, and the test results are shown in Table 1;

[0110] The test method for the flame retardant performance test is to take out five high flame retardant polypropylene fiber samples from Examples 1-12 and Comparative Examples 1-5 respectively, and then test the oxygen index of the above samples with reference to GB / T5454-1997 "Textile Combustion Performance Test Method Oxygen Index Method" and take the average value. The test results are shown in Table 1.

[0111]

[0112]

[0113] It can be seen from the above table that compared with comparative example 1, the elongation at break and the oxygen index of Examples 1-12 of the present invention are significantly improved; compared with comparative examples 1-5, when the corresponding different flame retardants and the content of other flame retardants are not added, the elongation at break and the oxygen index of Example 1 are different, wherein in comparative example 4, it is explained that the organic flame retardant and the inorganic flame retardant need to be used in combination to improve the flame retardant performance to a large extent; thus, it can be explained that the addition of decabromodiphenyl ether and antimony trioxide, the combination of organic flame retardant and inorganic flame retardant, and the addition of flame retardant can greatly improve the flame retardancy of polypropylene fiber on this basis, so that it has high flame retardant performance; wherein the oxygen index in Example 9 is the highest, indicating that the flame retardant performance obtained under the conditions of Example 9 is the best; therefore, the service life of polypropylene fiber products can be further extended and their scope of application can be expanded, and they can be used as a variety of industrial fabrics.

[0114] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A highly flame-retardant polypropylene fiber, characterized in that: The polypropylene fiber is composed of the following raw materials in parts by weight: 40-65 parts of polypropylene fiber chips and 35-60 parts of flame retardant masterbatch; wherein the flame retardant masterbatch is a mixture of 20-40 parts of decabromodiphenyl ether, 30-70 parts of antimony trioxide, 10-15 parts of flame retardant, 1-8 parts of antioxidant and 1-15 parts of coupling agent; the coupling agent is a mixture of polyethylene terephthalate bis(hydroxyethyl) resin and dioctyl pyrophosphate acyloxy, and the mass ratio of polyethylene terephthalate bis(hydroxyethyl) resin to dioctyl pyrophosphate acyloxy is 1:(2-5).

2. A highly flame-retardant polypropylene fiber as claimed in claim 1, characterized in that: The polypropylene fiber chips are 57 parts and the flame retardant masterbatch is 43 parts; wherein the flame retardant masterbatch is a mixture of 24 parts of decabromodiphenyl ether, 46 parts of antimony trioxide, 13 parts of flame retardant, 2 parts of antioxidant and 15 parts of coupling agent.

3. A highly flame-retardant polypropylene fiber as claimed in claim 1 or 2, characterized in that: The antioxidant is antioxidant 1010.

4. A highly flame-retardant polypropylene fiber as claimed in claim 1, characterized in that: The mass ratio of the polyethylene terephthalate resin to the dioctyl pyrophosphate acyloxy group is 1:2.

5.

5. A method for preparing a highly flame-retardant polypropylene fiber according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps S1, prepare a mixture, configure the ratio of polypropylene fiber chips and flame retardant masterbatch, place the configured polypropylene fiber chips and flame retardant masterbatch at a temperature of 90-105°C for preheating, and use a stirrer to continuously stir for 0.5-1h, cool at a temperature of 120-140°C, use a dryer for drying for 5-8h, and obtain a mixture; S2, obtaining a tow and completing shaping, conveying the mixture to a vacuum twin-screw extruder for melt extrusion to obtain a melt, filtering the melt through a filter and entering a melt pipe, and the melt after entering the melt pipe is spun through a spinneret of a spinning assembly to obtain a tow, and then shaping is performed; S3, subsequent processing, and subsequent shaping of the spinning, after cooling, drawing, curling, oiling, heat setting, cutting, and packaging, high flame retardant polypropylene fiber can be obtained.

6. The preparation method according to claim 5, characterized in that: The filter has a mesh size of 120-175 meshes.

7. The preparation method according to claim 5, characterized in that: In step S1, the preheating temperature is set to 100°C, and the stirring time t1 of the stirrer is 1h; and the cooling temperature is 135°C, and the drying time t2 is 6h.

Citation Information

Patent Citations

  • High-strength and flame-retardant hollow polypropylene fiber and preparation method thereof

    CN110331462A

Cited By

  • Production process of low-energy-consumption ribbon trademark material

    CN119243367A

  • High-strength polypropylene short fiber for cool cloth and preparation method of high-strength polypropylene short fiber

    CN121473015A