Printing and dyeing process of knitted fabric
Through the pretreatment, dyeing and color fixing process of knitted fabrics, hollow titanium dioxide nano microspheres modified by glycerol and 1,4-butanediol dye aid and coupling agent, the problem of printing and dyeing wastewater and insufficient dyeing fastness are solved. The problem of improving the color fastness and antibacterial properties of the fabric and expanding its scope of application.
Patent Information
- Application Number
- CN202411119246.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The wastewater generated during the printing and dyeing process is harmful to the environment. The dyeing fastness of existing knitted fabrics is poor and has a single function, and the scope of application is narrow.
Adopt the pretreatment, dyeing process and color fixing process of knitted fabrics, add environmentally friendly dye aids and wear-resistant and antibacterial color fixing liquid, including the use of glycerol and 1,4-butanediol as dye aids, and coupling agents Modified hollow titanium dioxide nano microspheres serve as a toner to improve color fastness and practicality.
It significantly improves the color fastness and friction resistance of knitted fabrics, reduces environmental pollution, expands its scope of application, and provides antibacterial effects.
Smart Images

Figure BDA0004994543570000081 
Figure BDA0004994543570000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of knitted fabrics, and in particular relates to a printing and dyeing process for knitted fabrics. Background Art
[0002] Knitted fabrics are made by bending yarns into loops and interlacing them with knitting needles. According to the weaving method, they are divided into two categories: weft knitted fabrics and warp knitted fabrics. Knitted fabrics have large gaps between yarns, are soft, absorbent, and have excellent elasticity and extensibility. Compared with woven fabrics, they have high production and are suitable for small batch production. Knitted fabrics are widely used in clothing fabrics, linings, home textiles and other products. Knitted clothing is soft, comfortable, close-fitting, and has no sense of tightness, and is deeply loved by consumers. Printing and dyeing, also known as dyeing and finishing, is a processing method, and is also a general term for pre-treatment, dyeing, printing, and finishing.
[0003] The wastewater generated by printing and dyeing is one of the most difficult industrial wastewaters to treat, and has a severe impact on the environment. It is necessary to reduce the addition of chemicals that are harmful to the environment from the source, that is, during the printing and dyeing process. Existing knitted fabrics have poor dye fastness and are easy to fade. After printing and dyeing, the fabrics have relatively single functions and a narrow range of applications. Summary of the invention
[0004] The object of the present invention is to provide a printing and dyeing process for knitted fabrics, wherein the knitted fabrics are printed and dyed through knitted fabric pretreatment, dyeing process, color fixing process and post-finishing process, wherein a dyeing auxiliary agent that does not pollute the environment is added in the dyeing process, and a wear-resistant and antibacterial color fixing liquid is added in the color fixing process, so as to improve the color fastness and practicality of the knitted fabrics.
[0005] The technical problem to be solved by the present invention is that the wastewater generated by printing and dyeing is one of the industrial wastewaters that is difficult to treat and has a relatively bad impact on the environment. It is necessary to reduce the addition of chemicals that are harmful to the environment from the source, that is, in the printing and dyeing process. The existing knitted fabrics have poor color fastness and are easy to fade. After finishing, the fabrics have a single function and a narrow scope of application. It is necessary to add a color fixing liquid to improve the color fastness of the knitted fabrics and at the same time improve the practicality of the knitted fabrics.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0008] A1. Pretreatment of knitted fabrics: Wash the knitted fabrics 2-3 times with deionized water, dry them, immerse them in NaOH solution for activation treatment, and dry them; the activation process exposes the hydroxyl groups of the knitted fabrics, improves their modification activity, and facilitates dyeing;
[0009] A2. Dyeing process: put active dye, dyeing auxiliary, sodium m-nitrobenzene sulfonate, sodium alginate paste and sodium bicarbonate into a dyeing tank, stir evenly, let stand to defoam, and prepare active dye paste; immerse the pretreated knitted fabric into the active dye paste for dyeing;
[0010] A3, color fixing process: immerse the dyed knitted fabric in a color fixing solution containing hollow titanium dioxide nano-microspheres modified by a coupling agent for color fixing;
[0011] A4. Finishing process: The knitted fabric after color fixation is sequentially dried, steamed, washed with cold water, soaped, washed with cold water, and dried.
[0012] Furthermore, the dyeing auxiliary is made of glycerol and 1,4-butanediol; the glycerol plays a hygroscopic role in the dyeing agent, can absorb as much water in the color paste as possible, help dissolve the dye, and depolymerize the dye polymer into dye single molecules, so that it is easier to immerse in the knitted fabric; the 1,4-butanediol can promote the swelling of the knitted fabric fiber, accelerate the diffusion and fixation of the dye into the fiber, and form a covalent bond with the fiber; glycerol and 1,4-butanediol are both environmentally friendly and can reduce the pollution of the environment by organic nitrogen-containing dyeing auxiliary.
[0013] Furthermore, the mass ratio of the glycerol to 1,4-butanediol is 1:0.5-4.
[0014] Furthermore, the sodium alginate paste is used as a thickener and is prepared by stirring pure sodium alginate and deionized water in a stirrer and standing to defoam.
[0015] Furthermore, the mass fraction ratio of the active dye, the dyeing auxiliary, the sodium m-nitrobenzene sulfonate, the sodium alginate paste and the sodium bicarbonate in the color paste is 5:5-10:1:70:3.
[0016] Furthermore, the preparation method of the color fixing solution is: mixing the coupling agent and anhydrous ethanol at 50-65°C, ultrasonically vibrating for 1 hour to obtain a modifier, and then adding hollow titanium dioxide nano-microspheres to the modifier, ultrasonically vibrating for 2.5-3 hours to obtain a color fixing solution, wherein the mass ratio of the coupling agent, anhydrous ethanol, and hollow titanium dioxide nano-microspheres is 2:1-3:26-40.
[0017] Furthermore, the method for preparing the hollow titanium dioxide nanospheres comprises the following steps:
[0018] B1. Dissolve glucose in deionized water, add ammonia water to make the solution pH reach 10, then add sodium polyacrylate, stir evenly and transfer into a reactor, then hydrothermally react at 160-180°C for 4h, cool, remove the precipitate in the reactor, centrifuge with deionized water and ethanol alternately for several times, and dry to obtain carbonaceous microspheres;
[0019] B2, dissolving titanium tetrachloride in a mixed solution of anhydrous ethanol and carbonaceous microspheres, ultrasonicating for 1 hour, stirring for 11 hours, then centrifuging alternately with deionized water and ethanol for several times, and drying to obtain a precursor;
[0020] B3. Place the precursor in a muffle furnace and heat it to 400-550°C at a heating rate of 5-10°C / min, keep it warm for 2 hours, and cool it to room temperature to obtain hollow titanium dioxide nanospheres.
[0021] During the above reaction process, glucose undergoes carbonization reaction and aggregates to form carbonaceous microspheres with a large number of oxygen-containing functional groups. These oxygen-containing functional groups will adsorb tetravalent titanium ions in the solution to form a precursor. When the precursor undergoes a step-by-step temperature increase calcination process, the C, H, and O elements on the surface of the precursor will be preferentially oxidized to CO2 and H2O, and the tetravalent titanium ions on the surface will be oxidized to titanium dioxide to form a titanium dioxide shell. The titanium dioxide shell and the core inside the precursor will generate a pair of opposite forces. Because of the existence of this pair of opposite forces, the sphere will not collapse. When this pair of forces reaches a critical condition, the shell will separate from the core to obtain hollow silica nanospheres.
[0022] Further, the coupling agent includes one or two of 3-aminopropyltrimethoxytitanate, γ-aminopropyltriethoxytitanate, 3-isocyanatopropyltriethoxytitanate or 3-glycidyloxypropyltrimethoxytitanate.
[0023] Beneficial effects of the present invention:
[0024] (1) In the technical solution of the present invention, the printing and dyeing agents used are environmentally friendly glycerol and 1,4-butanediol, which replace the organic nitrogen-containing printing and dyeing agents that are harmful to the environment, while also having the same dyeing effect as the organic nitrogen-containing printing and dyeing agents.
[0025] (2) In the technical solution of the present invention, in order to solve the problem that the color fastness of knitted fabrics is not enough and the application range is narrow, a layer of coupling agent modified hollow titanium dioxide nano-microsphere protective film with dual effects of wear resistance and antibacterial is fixed on the surface of the knitted fabric, so that the color fastness and friction fastness of the knitted fabric are greatly improved, and at the same time, the knitted fabric has excellent antibacterial effect. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0029] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0030] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:1), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0031] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and transfer to a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:13, ultrasonic oscillation was performed for 2.5 hours, and a fixing solution was obtained; A36, the cotton knitted fabric was immersed in the fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0032] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0033] Example 2
[0034] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0035] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0036] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:1), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0037] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and transfer to a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:15, and ultrasonic oscillation was performed for 2.5 hours to obtain a color fixing solution; A36, the cotton knitted fabric was immersed in the color fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0038] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0039] Example 3
[0040] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0041] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0042] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:1), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0043] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and transfer to a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nano-microspheres; A35, the hollow titanium dioxide nano-microspheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nano-microspheres was 1:17, and ultrasonic oscillation was performed for 2.5 hours to obtain a color fixing solution; A36, the cotton knitted fabric was immersed in the color fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0044] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0045] Example 4
[0046] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0047] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0048] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:1), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0049] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and transfer to a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:20, and ultrasonic oscillation was performed for 2.5 hours to obtain a color fixing solution; A36, the cotton knitted fabric was immersed in the color fixing solution, soaked for 1 hour with continuous stirring, and rolled dry;
[0050] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0051] Comparative Example 1
[0052] Compared with Examples 1, 2, 3 and 4, Comparative Example 1 was not subjected to the color fixing process, and other operations and conditions remained unchanged.
[0053] The color fixation rate, color fastness to rubbing, and antibacterial rate of the materials of Examples 1-4 and Comparative Example 1 are measured, and the measurement results are shown in Table 1 below.
[0054] Table 1
[0055]
[0056]
[0057] It can be seen from the data in Table 1 that the addition of the color fixing process greatly improves the color fixing rate, color fastness to rubbing and antibacterial rate of the knitted fabric. At the same time, with the increase of the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres, the color fixing rate and color fastness to rubbing of the knitted fabric first increase and then decrease, indicating that the color fixing rate and color fastness to rubbing are optimal when the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres is 1:17.
[0058] Example 5
[0059] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0060] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0061] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:0.5), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0062] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and move into a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:13, ultrasonically oscillated for 2.5 hours, and a fixing solution was obtained; A36, the cotton knitted fabric was immersed in the fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0063] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0064] Example 6
[0065] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0066] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0067] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:1), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0068] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and transfer to a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:13, ultrasonic oscillation was performed for 2.5 hours, and a fixing solution was obtained; A36, the cotton knitted fabric was immersed in the fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0069] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0070] Example 7
[0071] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0072] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0073] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:2), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0074] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and move into a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:13, ultrasonically oscillated for 2.5 hours, and a fixing solution was obtained; A36, the cotton knitted fabric was immersed in the fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0075] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0076] Example 8
[0077] A printing and dyeing process for knitted fabrics, comprising the following steps:
[0078] A1. Pretreatment of cotton knitted fabric: Wash the cotton knitted fabric three times with deionized water, dry it, immerse it in 0.2 mol / L NaOH solution for activation treatment, and dry it;
[0079] A2, dyeing process: 5wt% reactive brilliant red K-2BP, 5wt% glycerol and 1,4-butanediol (the mass ratio of glycerol to 1,4-butanediol is 1:3), 1wt% sodium m-nitrobenzene sulfonate, 70wt% sodium alginate paste, 3wt% sodium bicarbonate are put into a dyeing tank, the total amount of the color paste is 100g, stirred evenly, and allowed to stand for defoaming to obtain a reactive dye color paste; the pretreated cotton knitted fabric is immersed in the reactive dye color paste for dyeing, the temperature is raised to 60°C at a heating rate of 5°C / min, and the dyeing is carried out at a constant temperature for 20min;
[0080] A3. Fixing process: A31. Add 3-aminopropyltrimethoxytitanate to anhydrous ethanol and ultrasonically vibrate at 60°C for 1h to obtain a modifier; wherein the mass ratio of 3-aminopropyltrimethoxytitanate to anhydrous ethanol is 1:1; A32. Dissolve 5.6g of glucose in 40mL of deionized water, add ammonia water to make the solution pH reach 10, then add 2mg of sodium polyacrylate, stir evenly and move into a reactor, then react at 160°C for 4h, cool, remove the precipitate in the reactor, centrifuge it alternately with deionized water and ethanol for 3 times, and dry it to obtain carbonaceous microspheres; A33. Dissolve 0.9g of titanium tetrachloride in 40mL of anhydrous A34, the precursor was placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain hollow titanium dioxide nanospheres; A35, the hollow titanium dioxide nanospheres were dissolved in a modifier, the mass ratio of 3-aminopropyltrimethoxytitanium to hollow titanium dioxide nanospheres was 1:13, ultrasonically oscillated for 2.5 hours, and a fixing solution was obtained; A36, the cotton knitted fabric was immersed in the fixing solution, soaked for 1 hour and stirred continuously, and rolled dry;
[0081] A4. Finishing process: the knitted fabric after color fixation is dried at 100°C for 2 min, steamed at 102°C for 10 min, washed with cold water 20 times, then soaped at 90°C for 5 min at a detergent of 2081 g / L and a bath ratio of 1:50, then washed with cold water 10 times, and finally dried to obtain the dyed cotton knitted fabric.
[0082] Comparative Example 2
[0083] Compared with Examples 5, 6, 7 and 8, no dyeing aid was added in Comparative Example 2, and other conditions remained unchanged.
[0084] The dye uptake rates of the materials of Examples 5-8 and Comparative Example 2 are measured, and the measurement results are shown in Table 2 below.
[0085] Table 2
[0086] project Dyeing rate (%) Example 5 92.2 Example 6 93.5 Example 7 95.6 Example 8 92.4 Comparative Example 2 44.8
[0087] It can be seen from the data in Table 2 that the addition of dyeing auxiliaries significantly improves the dye uptake rate of knitted fabrics. At the same time, when the mass ratio of glycerol to 1,4-butanediol in the dyeing auxiliaries is 1:2, the dye uptake rate of knitted fabrics is the highest.
[0088] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0089] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A printing and dyeing process for knitted fabrics, It is characterized in that The following steps are involved: A1. Pretreatment of knitted fabrics: Wash the knitted fabrics 2-3 times with deionized water, dry them, immerse them in NaOH solution for activation treatment, and dry them; A2. Dyeing process: put active dye, dyeing auxiliary, sodium m-nitrobenzene sulfonate, sodium alginate paste and sodium bicarbonate into a dyeing tank, stir evenly, let stand to defoam, and prepare active dye paste; immerse the pretreated knitted fabric into the active dye paste for dyeing; A3, color fixing process: immerse the dyed knitted fabric in a color fixing solution containing hollow titanium dioxide nano-microspheres modified by a coupling agent for color fixing; A4. Finishing process: The knitted fabric after color fixation is sequentially dried, steamed, washed with cold water, soaped, washed with cold water, and dried.
2. A printing and dyeing process for knitted fabrics according to claim 1, It is characterized in that The dyeing auxiliary is prepared from glycerol and 1,4-butanediol.
3. A printing and dyeing process for knitted fabrics according to claim 2, It is characterized in that The mass ratio of the glycerol to 1,4-butanediol is 1:0.5-4.
4. The printing and dyeing process for knitted fabrics according to claim 1, It is characterized in that The sodium alginate original paste is prepared by stirring pure sodium alginate and deionized water in a stirrer and standing to defoam.
5. The printing and dyeing process for knitted fabric according to claim 1, It is characterized in that The mass fraction ratio of the active dye, the dyeing auxiliary, the sodium m-nitrobenzene sulfonate, the sodium alginate paste and the sodium bicarbonate in the color paste is 5:5-10:1:70:
3.
6. The printing and dyeing process for knitted fabric according to claim 1, It is characterized in that The preparation method of the color fixing solution is as follows: a coupling agent and anhydrous ethanol are mixed at 60-75° C., ultrasonically vibrated for 1 hour, and then hollow titanium dioxide nanospheres are added, and ultrasonically vibrated for 2.5-3 hours to obtain the color fixing solution.
7. A printing and dyeing process for knitted fabrics according to claim 6, It is characterized in that The method for preparing the hollow titanium dioxide nanospheres comprises the following steps: B1. Dissolve glucose in deionized water, add ammonia water to make the solution pH reach 10, then add sodium polyacrylate, stir evenly and transfer into a reactor, then react at 160-180°C for 4h, cool, remove the precipitate in the reactor, centrifuge with deionized water and ethanol alternately for several times, and dry to obtain carbonaceous microspheres; B2, dissolving titanium tetrachloride in a mixed solution of anhydrous ethanol and carbonaceous microspheres, ultrasonicating for 1 hour, stirring for 11 hours, then centrifuging alternately with deionized water and ethanol for several times, and drying to obtain a precursor; B3. Place the precursor in a muffle furnace and heat it to 400-550°C at a heating rate of 5-10°C / min, keep it warm for 2 hours, and cool it to room temperature to obtain hollow titanium dioxide nanospheres.
8. A printing and dyeing process for knitted fabrics according to claim 6, It is characterized in that The coupling agent includes one or two of 3-aminopropyl trimethoxy titanane, γ-aminopropyl triethoxy titanane, 3-isocyanatopropyl triethoxy titanane or 3-glycidyloxypropyl trimethoxy titanane.
9. The printing and dyeing process for knitted fabrics according to claim 6, It is characterized in that The mass ratio of the coupling agent, anhydrous ethanol and hollow titanium dioxide nano-microspheres is 2:1-3:26-40.