Temperature control method of oxyhydrogen flame and local annealing method of quartz product
Through the temperature control of hydrogen and oxygen flame and step-by-step cooling treatment, the local treatment problem in annealing of quartz glass products is solved, and efficient and low-cost local annealing is achieved, which is suitable for quartz glass products with complex structures.
Patent Information
- Application Number
- CN202411044905.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing annealing method of quartz glass products, high-temperature annealing furnace leads to overall softening and deformation, making it difficult to achieve local annealing. At the same time, the cost of laser annealing equipment is high and the local treatment of complex structures is limited.
Using the temperature control method of hydrogen and oxygen flame, the hydrogen and oxygen flame above 2500℃ is reduced to 800-1300℃. By setting up a mass flowmeter and a gas humidification device in the hydrogen and oxygen gas circuit, local annealing of quartz products is achieved, and the use of Step-by-step cooling treatment of hydrogen and oxygen flame.
Local annealing of quartz glass products is achieved, which avoids overall deformation, reduces costs, and improves processing efficiency. It is suitable for large-size or complex structures to treat quartz glass products, and is cooled at a lower temperature to avoid the generation of thermal stress.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0004973246510000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of quartz product production, and more specifically, to a temperature control method of an oxyhydrogen flame and a local annealing method of a quartz glass product. Background Art
[0002] Quartz glass is widely used in semiconductors, aerospace, optical communications and other fields due to its excellent high temperature resistance, cleanliness, corrosion resistance, light transmittance and filtering properties.
[0003] During the manufacturing process, cutting, grinding, thermal deformation and welding give it the desired shape and function, but also introduce residual stress, affecting performance. Annealing treatment is a key process, which eliminates stress and improves material stability and performance by precisely controlling heating, insulation and cooling. After annealing, the mechanical strength, optical properties and thermal stability of quartz glass products are significantly improved, meeting the strict requirements of high-end fields for material performance, and is an important link in ensuring product quality and competitiveness.
[0004] At present, the annealing treatment of quartz glass products is mostly carried out in a high-temperature annealing furnace. That is, the quartz glass product is placed in a high-temperature annealing furnace as a whole, heated to a temperature above the strain point of quartz at a fixed rate, and kept warm for a period of time to achieve the stress elimination effect, and then continued to cool at a fixed rate.
[0005] For example, publication number CN108383365A discloses a quartz glass annealing method, which includes four stages: a heating stage, a soaking stage, a slow cooling stage and a fast cooling stage. The quartz glass is stress-eliminated in an annealing furnace according to the above stages. The heating and soaking stages are mainly for stress-eliminated above the strain point of the quartz glass product; the slow cooling stage is mainly for preventing the quartz glass product from generating new stress after cooling, or reducing it to a required stress range; the fast cooling stage is for shortening the annealing process below the strain temperature of the product, reducing fuel consumption and improving productivity.
[0006] For example, publication number CN108675620A discloses a precision annealing method for quartz glass, which includes the following stages: a heating stage - a heat-averaging and heat-insulating stage - a slow cooling stage - a secondary heating stage - a secondary cooling stage. In the process of annealing the quartz glass, the secondary heating stage can further improve the temperature resistance of the quartz glass during use.
[0007] In addition, quartz glass products can also be annealed using lasers. Laser annealing is a method of irradiating the semiconductor surface with a laser beam to generate extremely high temperatures in the irradiated area, thereby repairing crystal damage and eliminating dislocations.
[0008] For example, publication number CN115527883A discloses a laser annealing device and annealing method, which uses pulsed laser and modulated waveform laser to cooperate with each other to perform laser annealing on the workpiece. The modulated waveform laser can preheat the annealing area of the workpiece, and the pulsed laser can quickly heat the annealing area of the workpiece. It can effectively activate the impurity ions in the shallow and deep layers of the workpiece and improve the annealing efficiency of the workpiece.
[0009] However, both high temperature annealing furnace and laser annealing have some problems.
[0010] Using a high-temperature annealing furnace for integrated annealing, on the one hand, will cause deformation of the quartz glass product due to overall softening, making it difficult to achieve local annealing; on the other hand, the surface of the quartz glass product after annealing is prone to serious metal impurity contamination.
[0011] The use of laser to anneal quartz glass products has the problem of expensive equipment and high cost. In addition, for quartz glass products with complex structures, it is difficult for laser to perform local annealing on special locations, which has certain limitations. Summary of the invention
[0012] The main purpose of the present invention is to provide a method for local annealing of a quartz product using an oxyhydrogen flame, and a method for controlling the temperature of the oxyhydrogen flame, so as to solve the technical problems mentioned in the background technology.
[0013] In order to solve the above technical problems, on the one hand, a temperature control method of oxyhydrogen flame is proposed, which reduces the temperature of oxyhydrogen flame above 2500℃ to 800-1300℃; the temperature control method is to set a mass flow meter in the gas path of hydrogen and oxygen, and adjust the combustion amount by controlling the gas flow in each gas path, thereby controlling the size and temperature of the flame.
[0014] In this technical solution, in order to achieve the goal of safely and stably reducing the oxyhydrogen flame from more than 2500℃ to 800-1300℃, the key lies in the precise control of the supply of hydrogen and oxygen. As the core component of this system, the mass flow meter monitors and adjusts the gas flow entering the gas path in real time through high-precision sensors. These flow meters not only have a high degree of measurement accuracy, but also can quickly respond to control signals to ensure that small changes in gas flow can be captured and adjusted immediately.
[0015] In the above technical solution, further, a gas humidifying device is provided in the hydrogen gas path to increase the humidity of the hydrogen.
[0016] In this technical solution, by increasing the humidity of hydrogen, the temperature of the flame combustion will be significantly reduced, thereby facilitating temperature control.
[0017] In any of the above technical solutions, further, the humidifying solution in the gas humidifying device is a pure organic solution.
[0018] In any of the above technical solutions, further, the pure organic solution is an alcohol aqueous solution.
[0019] In any of the above technical solutions, further, the alcohol aqueous solution is alcohol.
[0020] In any of the above technical solutions, further, the volume ratio of alcohol is 40-60vol%.
[0021] In any of the above technical solutions, further, the gas flow rates in the gas circuits of hydrogen and oxygen are both in the range of 1-2 L / min.
[0022] On the other hand, a local annealing method for a quartz product is also proposed, the annealing method comprising the following steps:
[0023] S1. Preheat the quartz product with oxyhydrogen flame at 800-1000℃ for a certain period of time;
[0024] S2, heating the preheated quartz product in a step-by-step manner;
[0025] S3, annealing the quartz product with oxyhydrogen flame at 1100-1200°C for a certain period of time;
[0026] S4, cooling the annealed quartz product in a step-by-step manner;
[0027] S5. Cool the cooled quartz product naturally.
[0028] On the other hand, a local annealing method for a quartz product is also proposed, the annealing method comprising the following steps:
[0029] S1. Use hydrogen-oxygen flame at 1100-1200℃ to directly anneal the quartz product for a certain period of time;
[0030] S2. Naturally cool the annealed quartz product.
[0031] In the above two technical solutions of the local annealing method of quartz products, further, the temperature control of the hydrogen-oxygen flame is achieved by controlling the flow rate of hydrogen and oxygen and the humidity of hydrogen;
[0032] The solution used to add humidity to the hydrogen is a pure organic solution.
[0033] Beneficial effects: Compared with the existing technology,
[0034] 1. The temperature control method of the present invention can control the temperature of the oxyhydrogen flame near the strain point of the quartz glass, and then the oxyhydrogen flame can be directly used with a welding gun to perform local annealing on the stress concentration part of the quartz glass product.
[0035] 2. The local annealing method of the present invention heats only the stress concentration part and does not affect the mechanical properties of other parts of the quartz glass product, so there is no risk of deformation of the entire quartz glass product.
[0036] 3. The gas used in the local annealing method of the present invention is of high purity and will not cause pollution to the surface of the quartz glass product during the annealing process;
[0037] 4. The local annealing method of the present invention is highly flexible and can be used to anneal quartz glass products of large size or complex structure.
[0038] 5. The local annealing method of the present invention adopts a stepped temperature, which allows the quartz glass product to be cooled at a lower temperature after annealing, thereby avoiding the generation of thermal stress.
[0039] 6. The local annealing method of the present invention can increase and decrease the temperature at a faster rate, thereby improving the processing efficiency.
[0040] 7. The local annealing method described in the present invention has simple and easy-to-obtain equipment, low cost, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 is a stress distribution diagram of the quartz glass sample before and after annealing in Example 3;
[0043] Figure 2 is a stress distribution diagram of the quartz glass sample before and after annealing in Example 4;
[0044] Figure 3 3 is a stress distribution diagram of the quartz glass sample in Example 6 before and after annealing. DETAILED DESCRIPTION
[0045] Below, the example embodiments according to the present application will be described in detail with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments of the present application, and it should be understood that the present application is not limited to the example embodiments described herein. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] It should be noted that, as shown in this application and claims, unless the context clearly indicates an exception, the words "a", "an", "a kind" and / or "the" do not specifically refer to the singular, but may also include the plural. Generally speaking, the terms "include" and "comprise" only indicate the inclusion of clearly identified steps and elements, and these steps and elements do not constitute an exclusive list, and the method or device may also include other steps or elements.
[0047] If the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0048] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0049] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0050] Oxyhydrogen flame is a flame produced by the combustion of hydrogen and oxygen mixed in a certain proportion. Since hydrogen and oxygen are both highly flammable gases, their mixed combustion can release huge energy, thus producing a high-temperature flame. This flame is not only high in temperature, but also pure and does not introduce impurities. Therefore, it is widely used in many fields, such as metal processing, quartz product processing, etc.
[0051] The normal temperature range of oxyhydrogen flame is generally 2500~3000℃, but for quartz, its melting point is about 1700℃. Therefore, in the quartz processing industry, the traditional method is generally to use oxyhydrogen flame to burn quartz products, and it is not used in annealing process. The main reason is that the temperature of oxyhydrogen flame is too high. A local annealing method of quartz products is proposed, which realizes the annealing of quartz glass products by using low-temperature oxyhydrogen flame.
[0052] The local annealing method and the temperature control method of the oxyhydrogen flame of the present application are described in detail through the following embodiments.
[0053] Embodiment 1:
[0054] In this embodiment, a temperature control method of an oxyhydrogen flame is proposed to reduce the temperature of the normal oxyhydrogen flame above 2500°C to 800-1300°C;
[0055] Among them, the temperature control method is to set a mass flow meter in the hydrogen and oxygen gas circuits, and adjust the combustion amount by controlling the gas flow in each gas circuit; a gas humidifying device is set in the hydrogen gas circuit, and the humidity of the hydrogen is increased by the gas humidifying device. Under the synergistic effect of the two methods, the size and temperature of the hydrogen-oxygen flame can be effectively controlled, so that it can be used for annealing treatment of quartz glass products.
[0056] It should be noted that hydrogen humidification will significantly reduce the flame combustion temperature of the hydrogen-oxygen flame.
[0057] It should be noted that the humidifying solution used in the gas humidification device is a pure organic solution. Pure organic solutions can be classified into
[0058] Water-based solution: Some organic substances can be dissolved in water to form water-based pure organic solutions, such as some alcohols, acids, sugars, etc.
[0059] Organic solvent solution: Most organic substances have high solubility in organic solvents, so organic solvents (such as ethanol, acetone, dimethyl sulfoxide, etc.) can be used as solvents to prepare pure organic solutions.
[0060] To save costs, an alcohol aqueous solution, such as alcohol, can be used as a humidifying solution. The hydrogen is humidified by the volatile alcohol.
[0061] The concentration of alcohol and the gas flow rates in the hydrogen and oxygen gas paths need to be strictly controlled to keep the temperature of the oxyhydrogen flame at 800-1300°C.
[0062] The following experiments were conducted on different alcohol concentrations and different flow rates of hydrogen and oxygen, and the following flame temperature table of hydrogen-oxygen flames was obtained.
[0063]
[0064]
[0065] The experiment found that alcohol solutions above 60 vol % would cause the flame to be unstable and easily extinguished, while alcohol solutions below 40 vol % would make it difficult to control the flame temperature below 1100°C.
[0066] According to the above experimental data, the alcohol solution is used as the humidifying solution when the volume ratio is in the range of 40-60vol%; when the gas flow rate range of hydrogen and oxygen in the gas path is controlled at 1-2L / min, the temperature of the hydrogen-oxygen flame can be controlled at 800-1300℃.
[0067] Preferably, 55 vol % alcohol solution and 60 vol % alcohol solution are used as the humidifying solution.
[0068] Embodiment 2:
[0069] This embodiment is a further improvement made on the basis of the first embodiment.
[0070] In this embodiment, a local annealing method for a quartz product is proposed, and the annealing method comprises the following steps:
[0071] S1. Preheat the quartz product with oxyhydrogen flame at 800-1000℃ for a certain period of time;
[0072] S2, heating the preheated quartz product in a step-by-step manner;
[0073] S3, annealing the quartz product with oxyhydrogen flame at 1100-1200°C for a certain period of time;
[0074] S4, cooling the annealed quartz product in a step-by-step manner;
[0075] S5. Cool the cooled quartz product naturally.
[0076] Different from high temperature annealing furnace, hydrogen oxygen flame acts directly on quartz glass products, and its heating rate is very fast. After the flame stops, the quartz glass products are directly exposed to room temperature air, and the cooling rate is also fast. In order to reduce the thermal stress that may be generated by the faster cooling rate, a step-by-step temperature rise annealing method is provided.
[0077] Embodiment three:
[0078] This embodiment is a further improvement made on the basis of the second embodiment.
[0079] The quartz glass products were annealed using a step-by-step heating and cooling method with a 60 vol % alcohol solution as the humidifying solution. The stress distribution of the quartz glass was tested using a fully automatic polarizing stress meter before and after annealing.
[0080] Step 1: first set the flow rate of hydrogen and oxygen to 1 L / min, refer to the table in Example 1, that is, use a flame of 804°C to preheat the quartz glass product, and keep the preheating for 5 minutes;
[0081] Step 2: After preheating, gradually increase the gas flow rate to 1.2 L / min, 1.4 L / min and 1.6 L / min, and maintain for 5 minutes respectively;
[0082] Step 3, finally using a gas flow rate of 1.8 L / min, i.e., a flame of 1191° C. to anneal the quartz glass product for 5 minutes;
[0083] Step 4: After annealing is completed, the gas flow rate is gradually reduced to 1.6 L / min, 1.4 L / min, 1.2 L / min and 1 L / min, and maintained for 5 minutes respectively. After the cooling is completed, the flame is turned off and the temperature is naturally cooled.
[0084] Step 5: Through the test of the fully automatic polarization stress meter, the average optical path difference of the quartz glass product before annealing is 2.146nm, and the average optical path difference of the quartz glass product after annealing is 1.336nm, which is reduced by 37.7%; Figure 1 As shown, the stress distribution of the quartz glass sample before and after annealing.
[0085] Embodiment 4:
[0086] This embodiment is a further improvement made on the basis of the second embodiment.
[0087] The quartz glass products were annealed using a step-wise heating and cooling method with 55 vol % alcohol solution as the humidifying solution. The stress distribution of the quartz glass was tested with a fully automatic polarizing stress meter before and after annealing.
[0088] Step 1: first set the flow rate of hydrogen and oxygen to 1 L / min, refer to the table in Example 1, that is, use a flame at 950°C to preheat the quartz glass product, and keep the preheating for 5 minutes;
[0089] Step 2: After preheating, gradually increase the gas flow rate to 1.2L / min and 1.4L / min, and maintain for 5 minutes respectively;
[0090] Step 3, finally using a gas flow rate of 1.6 L / min, i.e., a flame at 1180° C. to anneal the quartz glass product for 5 minutes;
[0091] Step 4: After annealing is completed, the gas flow rate is gradually reduced to 1.4 L / min, 1.2 L / min and 1 L / min, and maintained for 5 minutes respectively. After the cooling is completed, the flame is turned off and the temperature is naturally cooled.
[0092] Step 5: Through the test of the fully automatic polarization stress meter, the average optical path difference of the quartz glass product before annealing is 2.293nm, and the average optical path difference of the sample after annealing is 1.527nm, which is reduced by 33.4%; Figure 2 As shown, the stress distribution of the quartz glass sample before and after annealing.
[0093] Embodiment five:
[0094] The difference between this embodiment and the second embodiment is that another method is used to achieve local annealing of the quartz glass product.
[0095] In this embodiment, the annealing method includes the following steps:
[0096] S1. Use hydrogen-oxygen flame at 1100-1200℃ to directly anneal the quartz product for a certain period of time;
[0097] S2. Naturally cool the annealed quartz product.
[0098] Embodiment six:
[0099] This embodiment is a further improvement made on the basis of the fifth embodiment.
[0100] The quartz glass products were annealed by oxyhydrogen flame using 40 vol % alcohol solution as humidifying solution. The stress distribution of the quartz glass products was tested by a fully automatic polarizing stress meter before and after annealing.
[0101] Step 1: first set the flow rate of hydrogen and oxygen to 1 L / min, refer to the table in Example 1, that is, use a flame at 1158°C to directly anneal the quartz glass product for 10 minutes, and turn off the flame directly after the annealing to cool naturally.
[0102] Step 2: Through the test of the fully automatic polarization stress meter, the average optical path difference of the quartz glass product before annealing is 2.411nm, and the average optical path difference of the sample after annealing is 1.558nm, which is reduced by 26.8%; Figure 3 As shown, the stress distribution of the quartz glass sample before and after annealing.
[0103] The embodiments of the present disclosure have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for controlling the temperature of an oxyhydrogen flame, characterized in that: The temperature of the oxyhydrogen flame above 2500°C is reduced to 800-1300°C; the temperature control method is to set a mass flow meter in the hydrogen and oxygen gas paths, and adjust the combustion amount by controlling the gas flow in each gas path, thereby controlling the size and temperature of the flame.
2. The temperature control method of oxyhydrogen flame according to claim 1, characterized in that: A gas humidifying device is provided in the hydrogen gas path to increase the humidity of the hydrogen.
3. The temperature control method of oxyhydrogen flame according to claim 2, characterized in that: The humidifying solution in the gas humidifying device is an organic solution.
4. The temperature control method of oxyhydrogen flame according to claim 3, characterized in that: The organic solution is an alcohol aqueous solution.
5. The temperature control method of oxyhydrogen flame according to claim 4, characterized in that: The alcohol aqueous solution is an alcohol aqueous solution.
6. The temperature control method of oxyhydrogen flame according to claim 5, characterized in that: The volume ratio of the alcohol is 40-60 vol%.
7. The temperature control method of oxyhydrogen flame according to any one of claims 1 to 6, characterized in that: The gas flow rates in the gas lines of hydrogen and oxygen are both in the range of 1-2 L / min.
8. A method for local annealing of a quartz product, characterized in that: The annealing method comprises the following steps: S1. Preheat the quartz product with oxyhydrogen flame at 800-1000℃ for a certain period of time; S2, heating the preheated quartz product in a step-by-step manner; S3, annealing the quartz product with oxyhydrogen flame at 1100-1200°C for a certain period of time; S4, cooling the annealed quartz product in a step-by-step manner; S5. Cool the cooled quartz product naturally.
9. A method for local annealing of a quartz product, characterized in that: The annealing method comprises the following steps: S1. Use hydrogen-oxygen flame at 1100-1200℃ to directly anneal the quartz product for a certain period of time; S2. Naturally cool the annealed quartz product.
10. The local annealing method of a quartz glass product according to claim 8 or 9, characterized in that: The temperature control of the oxyhydrogen flame is achieved by controlling the flow rate of hydrogen and oxygen and the humidity of hydrogen; The solution used to add humidity to the hydrogen is an organic solution.
Citation Information
Patent Citations
Annealing method of quartz glass
CN108383365A
Precise quartz glass annealing method
CN108675620A
Laser annealing device and laser annealing method
CN115527883A