Method for evaluating cycle performance of lithium iron manganese phosphate positive electrode material

By performing a small charge and discharge cycle at high temperature and measuring the electrochemical impedance spectrum, the circulation performance of lithium manganese iron phosphate positive electrode material is quickly evaluated, which solves the problems of high cost and low efficiency of evaluation methods in the existing technology, and achieves high efficiency and accuracy Cycle performance evaluation.

CN118980720APending Publication Date: 2024-11-19HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411079089.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the cycling performance evaluation method of lithium manganese iron phosphate positive electrode material has high cost and low efficiency, and requires multiple charge and discharge cycles, which consumes a long time and increases time and equipment costs.

Method used

By performing a small charge and discharge cycle in a high temperature environment, the electrochemical impedance spectrum after initial charging and after cycling is determined, the charging resistance and cycling resistance are compared, and the impact of polarization, structural decay and electrolyte decomposition on cycling performance is indirectly characterized, and the phosphoric acid is quickly evaluated. Cycling properties of lithium iron manganese cathode material.

Benefits of technology

It reduces the time and equipment cost of cyclic performance evaluation, accelerates the R&D and production cycles, and can quickly judge the cyclic performance and structural differences of the positive electrode material, providing comprehensive and accurate evaluation results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980720A_ABST
    Figure CN118980720A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium batteries, and relates to a lithium manganese iron phosphate positive electrode material cycle performance evaluation method, which comprises: obtaining a standard lithium manganese iron phosphate positive electrode material and a to-be-tested positive electrode material; obtaining a standard battery and a to-be-tested battery respectively; carrying out activation and constant volume treatment on the battery; respectively charging to a first target voltage, respectively collecting electrochemical impedance spectrums of the battery after a first standing time, and respectively obtaining corresponding standard sample charging resistance and to-be-tested sample charging resistance; then charging and discharging circulation is carried out at a preset environment temperature, and corresponding standard sample circulation resistance and to-be-tested sample circulation resistance are obtained through electrochemical impedance spectroscopy of the battery after second standing time in a preset charge state; the standard sample charging resistance is compared with the to-be-tested sample charging resistance, the standard sample circulating resistance is compared with the to-be-tested sample circulating resistance, the circulating performance relation between the standard positive electrode material and the to-be-tested positive electrode material is judged according to comparison results, and evaluation time and equipment cost are greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium batteries, and in particular to a method for evaluating the cycle performance of lithium manganese iron phosphate positive electrode materials. Background Art

[0002] Lithium manganese iron phosphate positive electrode material has a higher theoretical energy density than lithium iron phosphate positive electrode material. In evaluating the various electrochemical properties of positive electrode materials, cycle performance is one of the most important indicators. At present, the main evaluation method for the cycle performance of positive electrode materials is to assemble them into batteries and perform multiple charge and discharge cycles, and evaluate the cycle performance of different batches of positive electrode materials by capacity retention rate. However, the methods of the prior art generally require hundreds or even thousands of cycles, such as 3,000 charge and discharge cycles at room temperature, each cycle lasting 3 hours; the evaluation methods of the prior art are time-consuming, which increases the time cost on the one hand, and on the other hand, the cycle test requires a long time to occupy the equipment, which increases the equipment cost and energy cost, thereby reducing the evaluation efficiency of the positive electrode material.

[0003] The existing technology has the problems of high cost and low efficiency in evaluating the cycle performance of lithium manganese iron phosphate positive electrode materials. Summary of the invention

[0004] The embodiment of the present application provides a method for evaluating the cycle performance of a lithium iron manganese phosphate positive electrode material, which aims to solve the problem of high cost and low efficiency of the method for evaluating the cycle performance of a lithium iron manganese phosphate positive electrode material to a certain extent.

[0005] In a first aspect, an embodiment of the present application provides a method for evaluating the cycle performance of a lithium iron manganese phosphate positive electrode material, comprising:

[0006] Obtain standard positive electrode materials of lithium manganese iron phosphate and positive electrode materials to be tested;

[0007] Based on the standard positive electrode material and the positive electrode material to be tested, a standard battery and a battery to be tested are prepared according to the same process respectively;

[0008] The standard battery and the battery to be tested are subjected to activation and constant capacity treatment under the same conditions;

[0009] The standard battery and the battery to be tested after the activation and constant capacity treatment are charged to a first target voltage respectively, and the electrochemical impedance spectra of the standard battery and the battery to be tested are collected respectively after being placed for a first static time to obtain the corresponding standard sample charging resistance and the sample to be tested charging resistance respectively;

[0010] The standard battery and the battery to be tested are respectively subjected to charge-discharge cycles at a preset ambient temperature, and electrochemical impedance spectra of the standard battery and the battery to be tested are respectively collected after being placed for a second rest time under a preset charge state, to obtain a standard sample cycle resistance corresponding to the preset charge state and a sample cycle resistance corresponding to the preset charge state;

[0011] The charging resistance of the standard sample and the charging resistance of the sample to be tested, the cycling resistance of the standard sample and the cycling resistance of the sample to be tested are compared respectively, and the cycling performance relationship between the standard positive electrode material of the lithium manganese iron phosphate positive electrode material and the positive electrode material to be tested is determined according to the comparison results.

[0012] The evaluation method of the cycle performance of the lithium iron manganese phosphate positive electrode material provided in the present application, compared with the prior art, is to quickly evaluate the cycle performance of the lithium iron manganese phosphate positive electrode material by measuring and comparing the charging resistance of the standard sample after charging and the charging resistance of the sample to be tested, and by measuring and comparing the standard sample cycle resistance and the sample cycle resistance of each preset charge state after the charge and discharge cycle in the preset ambient temperature, according to the comparison results. The main factors affecting the cycle performance of the lithium iron manganese phosphate positive electrode material are polarization, structural decay of the positive electrode material, and decomposition of the electrolyte during the long cycle. When the lithium iron manganese phosphate material battery is cycled and discharged in a high temperature environment of a preset ambient temperature, the higher ambient temperature will promote the decomposition of the electrolyte, forming a thicker surface film layer on the surface of the lithium iron manganese phosphate positive electrode, and also promote the dissolution of manganese and iron ions in the lithium iron manganese phosphate, resulting in structural decay and loss of active lithium; in addition, the "Jahn-Teller" effect side reaction produced by the manganese element in the lithium iron manganese phosphate will also be catalyzed to a certain extent at high temperature, and these factors will accelerate the battery capacity decay. By testing the electrochemical impedance spectroscopy (EIS) of a battery made of lithium manganese iron phosphate positive electrode material at each preset charge state after initial charging and cyclic charge and discharge, the degree to which the positive electrode material is affected by polarization can be directly characterized.

[0013] The evaluation method of the cycle performance of the lithium iron manganese phosphate positive electrode material of the present application only needs to perform a small amount of charge and discharge cycles at a relatively high ambient temperature for data collection. The resistance of the positive electrode material after initial charging and the resistance of different preset charge states after cyclic charge and discharge directly reflect the degree of influence of polarization on the positive electrode material. The electrochemical impedance spectroscopy data collected after short-term cycling at high temperature are used to indirectly characterize the influence of electrolyte decomposition, manganese and iron ion dissolution and active lithium loss on the cycle performance of the lithium iron manganese phosphate positive electrode material, thereby efficiently evaluating the cycle performance of the lithium iron manganese phosphate positive electrode material, and the evaluation results are comprehensive and accurate, thereby greatly reducing the evaluation time and equipment cost of the cycle performance, and accelerating the research and development and production cycle. In addition, by testing the cycle performance of the lithium iron manganese phosphate material at high temperature, the differences in the structure of the positive electrode material coating layer and the like can be quickly judged, and the evolution of these factors can be indirectly characterized in combination with the electrochemical impedance spectroscopy test. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0015] Figure 1 It is a schematic flow chart of a method for evaluating the cycle performance of lithium iron manganese phosphate positive electrode material provided in one embodiment of the present application;

[0016] Figure 2 The positive electrode material 1 (denoted as LFMP) of lithium iron manganese phosphate to be tested in Example 1 of the present application A ) and standard cathode materials (LFMPs) after charging.

[0017] Figure 3 It is a schematic diagram of an equivalent circuit of the electrochemical reaction process at the electrode-electrolyte interface in the battery of the present application;

[0018] Figure 4 It is the LFMP of Example 1 of the present application A Schematic diagram of the capacity retention rate and constant current charging ratio of batteries made of LFMPs after 25 cycles at 1C at 45°C;

[0019] Figure 5 It is the LFMP of Example 1 of the present application A Electrochemical impedance spectra of batteries made of LFMPs and LFMPs after 25 cycles at 1C at 45°C;

[0020] Figure 6The positive electrode material 1 (denoted as LFMP) of lithium iron manganese phosphate to be tested in Example 2 of the present application A ) and standard cathode materials (LFMPs) after charging.

[0021] Figure 7 It is the LFMP of Example 2 of the present application A Electrochemical impedance spectra of batteries made of LFMPs and LFMPs after 15 cycles at 1C at 35°C;

[0022] Figure 8 The positive electrode material 2 (denoted as LFMP) of lithium iron manganese phosphate to be tested in Example 3 of the present application B ) and standard cathode materials (LFMPs) after charging.

[0023] Fig. 9 It is the LFMP of Example 3 of the present application B Electrochemical impedance spectra of batteries made of LFMPs and LFMPs after 25 cycles at 1C at 45°C;

[0024] Fig.10 It is the LFMP of the comparative example of this application A LFMP B Electrochemical impedance spectroscopy of LFMPs after 500 cycles at 25 °C. DETAILED DESCRIPTION

[0025] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0026] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0027] In the present application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0028] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0029] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0030] It should be understood that in the various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0031] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0034] State of charge, also known as remaining capacity, is the full name of State of Charge, hereinafter referred to as SOC, which represents the ratio of the remaining capacity of the battery after a period of use or long-term storage to its fully charged capacity, usually expressed as a percentage. Its value range is 0-100%. When SOC=0, it means that the battery is fully discharged, and when SOC=100%, it means that the battery is fully charged.

[0035] Lithium manganese iron phosphate positive electrode material has a higher theoretical energy density than lithium iron phosphate positive electrode material. In evaluating the various electrochemical properties of positive electrode materials, cycle performance is one of the most important indicators. At present, the main evaluation method for the cycle performance of positive electrode materials is to assemble them into batteries and perform multiple full charge and discharge cycles, and evaluate the cycle performance of different batches of positive electrode materials by capacity retention rate. However, the methods of the prior art generally require hundreds or even thousands of cycles, such as 500 to 3000 charge and discharge cycles at room temperature, and each cycle takes 3 hours; the evaluation methods of the prior art are time-consuming, which increases the time cost on the one hand, and on the other hand, the cycle test requires a long time to occupy the equipment, which increases the equipment cost and energy cost, thereby reducing the evaluation efficiency of the positive electrode material.

[0036] In order to overcome the above technical problems to a certain extent, Figure 1 As shown, the first aspect of the embodiment of the present application provides a method for evaluating the cycle performance of a lithium manganese iron phosphate positive electrode material, comprising:

[0037] S1, obtaining a standard positive electrode material of lithium manganese iron phosphate and a positive electrode material to be tested.

[0038] S2, preparing a standard battery and a battery to be tested based on the standard positive electrode material and the positive electrode material to be tested respectively according to the same process.

[0039] S3, activating and fixing the capacity of the standard battery and the battery to be tested under the same conditions.

[0040] S4, charging the standard battery and the battery to be tested after activation and constant capacity treatment to a first target voltage respectively, and collecting electrochemical impedance spectra of the standard battery and the battery to be tested respectively after a first resting time, and obtaining corresponding standard sample charging resistance and test sample charging resistance respectively.

[0041] S5, subjecting the standard battery and the battery to be tested to charge and discharge cycles at a preset ambient temperature, and collecting electrochemical impedance spectra of the standard battery and the battery to be tested after a second rest time at a preset charge state, to obtain a standard sample cycle resistance corresponding to the preset charge state and a sample cycle resistance corresponding to the preset charge state.

[0042] S6, respectively comparing the charging resistance of the standard sample and the charging resistance of the sample to be tested, and the cycling resistance of the standard sample and the cycling resistance of the sample to be tested, and judging the cycling performance relationship between the standard positive electrode material of the lithium manganese iron phosphate positive electrode material and the positive electrode material to be tested according to the comparison results.

[0043] The evaluation method of the cycle performance of the lithium iron manganese phosphate positive electrode material provided in the present application, compared with the prior art, is to quickly evaluate the cycle performance of the lithium iron manganese phosphate positive electrode material by measuring and comparing the charging resistance of the standard sample after charging and the charging resistance of the sample to be tested, and by measuring and comparing the standard sample cycle resistance and the sample cycle resistance of each preset charge state after the charge and discharge cycle in the preset ambient temperature, according to the comparison results. The main factors affecting the cycle performance of the lithium iron manganese phosphate positive electrode material are polarization, structural decay of the positive electrode material, and decomposition of the electrolyte during the long cycle. When the lithium iron manganese phosphate material battery is cycled and discharged in a high temperature environment of a preset ambient temperature, the higher ambient temperature will promote the decomposition of the electrolyte, forming a thicker surface film layer on the surface of the lithium iron manganese phosphate positive electrode, and also promote the dissolution of manganese and iron ions in the lithium iron manganese phosphate, resulting in structural decay and loss of active lithium; in addition, the "Jahn-Teller" effect side reaction produced by the manganese element in the lithium iron manganese phosphate will also be catalyzed to a certain extent at high temperature, and these factors will accelerate the battery capacity decay. The degree to which the positive electrode material is affected by polarization can be directly characterized by testing the electrochemical impedance spectroscopy (EIS) of the battery prepared with lithium manganese iron phosphate positive electrode material at each preset charge state after initial charging and cyclic charge and discharge. Among them, polarization (including ohmic polarization, electrochemical polarization and concentration polarization) will cause the electrode potential to shift; structural degradation is manifested as the dissolution of manganese and iron ions in the positive electrode material, resulting in the loss of active lithium; and the decomposition of the electrolyte will form a thicker surface film layer on the surface of the lithium manganese iron phosphate positive electrode, indirectly causing polarization to increase.

[0044] The evaluation method of the cycle performance of the lithium iron manganese phosphate positive electrode material of the present application only needs to perform a small amount of charge and discharge cycles at a relatively high ambient temperature for data collection. The resistance of the positive electrode material after initial charging and the resistance of different preset charge states after cyclic charge and discharge directly reflect the degree of influence of polarization on the positive electrode material. The electrochemical impedance spectroscopy data collected after short-term cycling at high temperature are used to indirectly characterize the influence of electrolyte decomposition, manganese and iron ion dissolution and active lithium loss on the cycle performance of the lithium iron manganese phosphate positive electrode material, thereby efficiently evaluating the cycle performance of the lithium iron manganese phosphate positive electrode material, and the evaluation results are comprehensive and accurate, thereby greatly reducing the evaluation time and equipment cost of the cycle performance, and accelerating the research and development and production cycle. In addition, by testing the cycle performance of the lithium iron manganese phosphate material at high temperature, the differences in the structure of the positive electrode material coating layer and the like can be quickly judged, and the evolution of these factors can be indirectly characterized in combination with the electrochemical impedance spectroscopy test.

[0045] The main function of activation and volume setting is to enable the active substances of the electrode materials to fully participate in the reaction and reach an optimal state. After the activation treatment, the capacity remains unchanged at the maximum value under the activation current, indicating that the activation is complete. Generally, the newly assembled battery may cause slow electrochemical reaction and incomplete capacity release due to insufficient contact between the electrolyte and the electrode active substances. The resistances tested by the electrochemical impedance spectroscopy may be too large. If the cycle test is conducted directly without activation, it may be activated in the first few cycles, so the electrochemical impedance spectroscopy data of the test will be inaccurate. Generally, the smaller the activation current, the more complete the activation.

[0046] In some embodiments, the activation and constant capacity treatment in step S3 includes: charging the battery to be tested and the standard battery to a second target voltage with constant current and constant voltage, and placing them for a third rest time; discharging the battery to be tested and the standard battery to a third target voltage with constant current, and then placing them for a fourth rest time. According to the activation and constant capacity treatment method in this embodiment, the maximum capacity of the battery to be tested and the standard battery can be increased, and the electrochemical impedance spectrum error caused by the production process of the battery to be tested and the standard battery can be reduced.

[0047] In some embodiments, the activation and constant-capacity treatment is performed for 1 to 5 cycles; and / or, the second target voltage is 3.7V to 4.3V; and / or, the third target voltage is 1.8V to 2.0V; and / or, the third resting time and the fourth resting time are both 5min to 30min; and / or, constant-current and constant-voltage charging and constant-current discharging are both performed under 0.01C to 0.1C conditions. According to the conditional activation and constant-capacity treatment of this embodiment, the sufficiency of the electrochemical reaction of the battery can be improved, the maximum capacity of the battery to be tested and the standard battery can be improved, and the electrochemical impedance spectrum error caused by the production process of the battery to be tested and the standard battery can be further reduced.

[0048] In some embodiments, the criterion for judging the relationship between the cycle performance of the standard positive electrode material of the lithium iron manganese phosphate positive electrode material and the positive electrode material to be tested is: if the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample, and the cycle resistances of each sample to be tested are greater than the cycle resistances of each standard sample, then the cycle performance of the positive electrode material to be tested of the lithium iron manganese phosphate positive electrode material is judged to be lower than the cycle performance of the standard positive electrode material; if the charging resistance of the sample to be tested is less than the charging resistance of the standard sample, and the cycle resistances of each sample to be tested are less than the cycle resistances of each standard sample, then the cycle performance of the positive electrode material to be tested of the lithium iron manganese phosphate positive electrode material is judged to be higher than the cycle performance of the standard positive electrode material. According to the judgment criterion of this embodiment, the relationship between the cycle performance of the positive electrode material to be tested and the cycle performance of the standard positive electrode material is determined by judging the size of the charging resistance of the sample to be tested and the charging resistance of the standard sample and the cycle resistances of each sample to be tested and the cycle resistances of each standard sample, thereby reducing the cost of determining the cycle performance of the two materials.

[0049] In some embodiments, the preset state of charge includes a first state of charge, a second state of charge, a third state of charge, and a fourth state of charge, the standard sample circulation resistance includes a first standard sample circulation resistance corresponding to the first state of charge, a second standard sample circulation resistance corresponding to the second state of charge, a third standard sample circulation resistance corresponding to the third state of charge, and a fourth standard sample circulation resistance corresponding to the fourth state of charge, and the sample circulation resistance to be tested includes a first sample circulation resistance to be tested corresponding to the first state of charge, a second sample circulation resistance to be tested corresponding to the second state of charge, a third sample circulation resistance to be tested corresponding to the third state of charge, and a fourth sample circulation resistance to be tested corresponding to the fourth state of charge; wherein, the first state of charge < the second state of charge < the third state of charge < the fourth state of charge. In this embodiment, the corresponding standard sample circulation resistance and the sample circulation resistance to be tested are determined according to the four states of charge, the measurement conditions of the circulation resistance are further clarified, and the accuracy of the circulation resistance in characterizing the positive electrode material is improved.

[0050] In some embodiments, the first state of charge is 5% to 15%, the second state of charge is 75% to 85%, the third state of charge is 92.5% to 97.5%, and the fourth state of charge is 100%. This embodiment limits the range of each state of charge, thereby further clarifying the measurement conditions of the charge state corresponding to the cycle resistance, and improving the accuracy of the cycle resistance in characterizing the positive electrode material for preparing the battery.

[0051] In some embodiments, if the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample and the cycle resistance of the sample to be tested is greater than the cycle resistance of the standard sample, then it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is lower than the cycle performance of the standard positive electrode material, including:

[0052] If the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample, the cycling resistance of the first sample to be tested is greater than the cycling resistance of the first standard sample, the cycling resistance of the second sample to be tested is greater than the cycling resistance of the second standard sample, the cycling resistance of the third sample to be tested is greater than the cycling resistance of the third standard sample, and the cycling resistance of the fourth sample to be tested is greater than the cycling resistance of the fourth standard sample, then it is determined that the cycling performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is lower than the cycling performance of the standard positive electrode material.

[0053] In this embodiment, by judging the size relationship between one group of charging resistance and four groups of cycle resistance of the positive electrode material to be tested and the standard positive electrode material, the relationship between the cycle performance of the positive electrode material to be tested and the cycle performance of the standard positive electrode material is determined, thereby reducing the cost of determining the cycle performance of the two materials.

[0054] In some embodiments, if the charging resistance of the sample to be tested is less than the charging resistance of the standard sample and the cycle resistance of the sample to be tested is less than the cycle resistance of the standard sample, then it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is higher than the cycle performance of the standard positive electrode material, including:

[0055] If the charging resistance of the sample to be tested is smaller than the charging resistance of the standard sample, the cycling resistance of the first sample to be tested is smaller than the cycling resistance of the first standard sample, the cycling resistance of the second sample to be tested is smaller than the cycling resistance of the second standard sample, the cycling resistance of the third sample to be tested is smaller than the cycling resistance of the third standard sample, and the cycling resistance of the fourth sample to be tested is smaller than the cycling resistance of the fourth standard sample, then it is determined that the cycling performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is higher than the cycling performance of the standard positive electrode material.

[0056] In this embodiment, by judging the size relationship between one group of charging resistance and four groups of cycle resistance of the positive electrode material to be tested and the standard positive electrode material, the relationship between the cycle performance of the positive electrode material to be tested and the cycle performance of the standard positive electrode material is determined, thereby reducing the cost of determining the cycle performance of the two materials.

[0057] In some embodiments, the first resting time is 0.5h to 2h, and the second resting time is 1.0h to 5.0h; and / or, the charge-discharge cycle is performed for 10 to 30 cycles at 0.5C to 5C. According to the limiting conditions of this embodiment, measuring the charge resistance and the cycle resistance after resting can reduce the electrochemical reaction of the battery and improve the accuracy of the charge resistance and the cycle resistance; limiting the current conditions and the number of cycles of the charge-discharge cycle is conducive to setting the current according to the needs of the specific battery and reducing the time cost of evaluating the cycle performance.

[0058] In some embodiments, the preset ambient temperature is 25°C to 60°C; and / or, charging to the first target voltage is performed under 0.01C to 0.1C, and the first target voltage is 3.7V to 4.2V. According to the preset ambient temperature defined in this embodiment, since the temperature for evaluating the cycle performance is higher than the room temperature, the aging rate of the battery cycle performance is accelerated, thereby reducing the time cost of the evaluation; the charging current condition and the target voltage are limited to ensure that the battery is charged to the saturated capacity, which is convenient for testing the initial charging resistance and improves the accuracy of measuring the charging resistance.

[0059] In some embodiments, the polarization voltage of the electrochemical workstation used to collect the electrochemical impedance spectrum is 10 mV, and the frequency is 0.001 Hz to 100,000 Hz; limiting the working conditions of the electrochemical workstation improves the accuracy of measuring the charging resistance and the cycle resistance.

[0060] The technical solution of the present application is illustrated below through specific embodiments and comparative examples.

[0061] Example 1

[0062] Step 1), the positive electrode material 1 to be tested of lithium iron manganese phosphate (referred to as LFMP A) and standard positive electrode materials (LFMPs) were assembled into a test battery 1 and a standard battery under the same conditions and in the same process, and the test battery 1 and the standard battery were left to stand for 12 hours. After the electrolyte of the test battery 1 and the standard battery was fully infiltrated, they were respectively charged and discharged for 3 cycles in the battery test system to activate and fix the volume. Among them, the activation and fixing volume step includes: charging the test battery 1 and the standard battery to 4.3V at 0.1C constant current and constant voltage, standing for 10 minutes, and then discharging to 2.0V at 0.1C constant current and standing for 10 minutes.

[0063] Step 2), the activated battery 1 to be tested and the standard battery are charged to 4.3V at a constant current and constant voltage of 0.1C respectively, and the initial electrochemical impedance spectra (EIS) of the battery 1 to be tested and the standard battery are collected after standing for 1 hour, and the corresponding charging resistance 1 of the test sample and the charging resistance of the standard sample are obtained respectively;

[0064] Step 3), then the battery 1 to be tested and the standard battery are subjected to 25 cycles of charge and discharge at 1C current at an ambient temperature of 45°C, respectively. After standing for 3 hours at a state of charge of 100%, the electrochemical impedance spectra (EIS) of the battery 1 to be tested and the standard battery are collected to obtain the test sample cycle resistance 1 and the standard sample cycle resistance corresponding to the charge state of 0%, respectively.

[0065] Theoretically, the electrochemical reaction process at the electrode-electrolyte interface can be divided into three stages: diffusion, adsorption, and charge transfer. In the reaction process of lithium manganese iron phosphate electrode materials, the solvated lithium ions in the electrolyte first diffuse to the electrode-electrolyte interface, and then adsorb on the electrode material, and then the redox reaction occurs.

[0066] Figure 2 The positive electrode material 1 to be tested is lithium iron manganese phosphate (denoted as LFMP A ) and standard cathode materials (LFMPs) after charging, where the abscissa is the real part of the impedance at different frequencies, and the ordinate is the imaginary part of the impedance at different frequencies; Figure 2 Medium LFMP A The initial charging electrochemical impedance spectra of the positive electrode materials of LFMPs and LFMPs are composed of two semicircles in the high-frequency region and an oblique straight line in the low-frequency region. The two semicircles in the high-frequency region indicate that there are two parallel electrochemical reactions in the electrode process, which correspond to the charge transfer (Rct1) and electroadsorption (Rct2) processes respectively. The straight line in the low-frequency region corresponds to the diffusion process. The intercept of the electrochemical impedance spectrum curve on the horizontal axis represents the equivalent series resistance (Rs) caused by the material itself and contact. Figure 3 It is the equivalent circuit diagram of the electrochemical reaction process at the electrode-electrolyte interface in the battery. Figure 3The curve of the electrochemical impedance spectrum was fitted with the equivalent circuit diagram, and the results of each fitting resistance are shown in Table 1.

[0067] Table 1 LFMP A The initial charge resistance and the cycle resistance of LFMPs with a charge state of 100% after 25 cycles at 45 °C are fitted.

[0068]

[0069] Among them, after charging to 4.3V, the LFMPs charging resistors Rs, Rct1 and Rct2 are 1.04Ω, 5.47Ω and 6.88Ω respectively; A The charging resistors Rs, Rct1 and Rct2 are 1.2Ω, 5.76Ω and 6.97Ω respectively, LFMP A The resistance values ​​of each part are slightly larger than LFMPs, indicating that LFMP A More affected by polarization.

[0070] Figure 4 For LFMP A The capacity retention rate and constant current charging ratio of the batteries made of LFMPs and LFMPs after 25 cycles at 1C at 45°C. After 25 cycles, the capacity retention rate is 100%, but the LFMP A The constant current charging ratio of the batteries made of LFMPs and LFMPs decreased gradually during 25 cycles, among which, the constant current charging ratio of the battery made of LFMPs decreased to 97.11%, and that of the battery made of LFMPs decreased to 97.11%. A The result of the manufactured battery dropped to 95.89%, which indicates that the charging potential platform of the battery deviates more and more from the working potential during the cycle process, and the polarization deepens accordingly.

[0071] Figure 5 For LFMP A The electrochemical impedance spectra of the batteries made of LFMPs and LFMPs after 25 cycles at 1C at 45°C. In Table 1, when the state of charge is 100% after 25 cycles at 45°C, the Rs, Rct1 and Rct2 of the fourth standard sample of LFMPs are 4.4Ω, 35.6Ω and 13.18Ω respectively; A The fourth sample to be tested has a loop resistance of Rs, Rct1 and Rct2 of 5.8Ω, 38.0Ω and 14.3Ω respectively, LFMP A The resistance values ​​of each part are slightly larger than LFMPs, indicating that LFMP A More affected by polarization;

[0072] Under high temperature environment, the dissolution of manganese and iron ions in lithium manganese iron phosphate material and the decomposition of electrolyte are accelerated, resulting in the destruction of the lithium manganese iron phosphate structure and the thickening of the surface film layer, which indirectly leads to the attenuation of battery capacity.

[0073] Table 2 shows the resistance fitting values ​​of the cyclic resistances of LFMPA and LFMPs at charge states of 10%, 80% and 95% after 25 cycles at 45°C, that is, after 25 cycles, the battery is discharged to charge states of 10%, 80% and 95%, respectively, and then the cyclic resistance is determined.

[0074] Table 2 LFMP A The resistance fitting values ​​of the cyclic resistance of LFMPs with charge states of 10%, 80% and 95% after 25 cycles at 45℃

[0075]

[0076] In summary, LFMP A The cycling performance of the cathode material is lower than that of the LFMPs cathode material.

[0077] Example 2: The difference from Example 1 is that the number of activation cycles in step 1) is set to 4, the preset ambient temperature in step 3) is set to 35°C, and the number of charge and discharge cycles is set to 15.

[0078] Figure 6 The positive electrode material 1 to be tested is lithium iron manganese phosphate (denoted as LFMP A ) and standard positive electrode materials (LFMPs) after charging, wherein the abscissa is the real part of the impedance at different frequencies, and the ordinate is the imaginary part of the impedance at different frequencies; the curve of the electrochemical impedance spectrum is fitted according to the equivalent circuit diagram, and the results of each fitting resistance are shown in Table 3.

[0079] As shown in Table 3, after charging to 4.3 V, the LFMPs charging resistors Rs, Rct1, and Rct2 are 1.05Ω, 5.46Ω, and 6.87Ω, respectively; A The charging resistors Rs, Rct1 and Rct2 are 1.19Ω, 5.75Ω and 6.99Ω respectively, LFMP A The resistance values ​​of each part are slightly larger than LFMPs, indicating that LFMP A More affected by polarization.

[0080] Figure 7 For LFMP A The electrochemical impedance spectra of the batteries made of LFMPs and LFMPs after 15 cycles at 1C at 35°C. In Table 3, when the state of charge is 100% after 15 cycles at 35°C, the Rs, Rct1 and Rct2 of the fourth standard sample of LFMPs are 3.2Ω, 19.7Ω and 7.15Ω respectively; AThe fourth sample to be tested has a circulating resistance of Rs, Rct1 and Rct2 of 5.1Ω, 25.4Ω and 9.09Ω respectively, LFMP A The resistance values ​​of each part are slightly larger than LFMPs, indicating that LFMP A More affected by polarization.

[0081] Table 3 LFMP A The initial charge resistance of LFMPs and the cycle resistance with a charge state of 100% after 15 cycles at 35°C are fitted.

[0082]

[0083] Table 4 shows the resistance fitting values ​​of the cyclic resistances of LFMPA and LFMPs at charge states of 10%, 80% and 95% after 25 cycles at 45°C.

[0084] Table 4 LFMP A The resistance fitting values ​​of the cyclic resistance of LFMPs with charge states of 10%, 80% and 95% after 15 cycles at 35℃

[0085]

[0086] In summary, LFMP A The cycling performance of the cathode material is lower than that of the LFMPs cathode material.

[0087] Example 3: The difference from Example 1 is that the positive electrode material of lithium iron manganese phosphate is replaced with the positive electrode material 2 to be tested (referred to as LFMP B ), all parameters are the same.

[0088] Figure 8 The positive electrode material 2 to be tested is lithium iron manganese phosphate (denoted as LFMP B ) and standard positive electrode materials (LFMPs) after charging, wherein the abscissa is the real part of the impedance at different frequencies, and the ordinate is the imaginary part of the impedance at different frequencies; the curve of the electrochemical impedance spectrum is fitted according to the equivalent circuit diagram, and the results of each fitting resistance are shown in Table 5.

[0089] As shown in Table 5, after charging to 4.3 V, the LFMPs charging resistors Rs, Rct1, and Rct2 are 1.04Ω, 5.47Ω, and 6.88Ω, respectively; B The charging resistors Rs, Rct1 and Rct2 are 0.92Ω, 5.29Ω and 6.75Ω respectively, LFMP B The resistance values ​​of each item are slightly smaller than LFMPs, indicating that LFMP B Less affected by polarization.

[0090] Fig. 9 For LFMP B The electrochemical impedance spectra of the batteries made of LFMPs and LFMPs after 25 cycles at 1C at 45°C. In Table 3, when the state of charge is 100% after 25 cycles at 45°C, the Rs, Rct1 and Rct2 of the fourth standard sample of LFMPs are 4.4Ω, 35.6Ω and 13.18Ω respectively; A The fourth sample to be tested has a loop resistance of Rs, Rct1 and Rct2 of 3.6Ω, 33.7Ω and 12.0Ω respectively, LFMP B The resistance values ​​of each item are slightly smaller than LFMPs, indicating that LFMP A Less affected by polarization.

[0091] Table 5 LFMP B The initial charge resistance and the cycle resistance of LFMPs with a charge state of 100% after 25 cycles at 45 °C are fitted.

[0092]

[0093] Table 6 shows the LFMP B The resistance fitting values ​​of the cyclic resistances of LFMPs with charge states of 10%, 80% and 95% after 25 cycles at 45°C.

[0094] Table 6LFMP B The resistance fitting values ​​of the cyclic resistance of LFMPs with charge states of 10%, 80% and 95% after 25 cycles at 45℃

[0095]

[0096] In summary, LFMP A The cycle performance of the cathode material is higher than that of LFMPs cathode material.

[0097] Comparative Example 1: The difference from Example 1 is that the positive electrode material 1 to be tested of lithium iron manganese phosphate (referred to as LFMP A ) and the positive electrode material 2 to be tested (denoted as LFMP B ) were subjected to 300 and 500 charge-discharge cycles at 1C with the standard cathode material (LFMPs), and the ambient temperature of the charge-discharge cycle was 25°C.

[0098] Fig.10 For LFMP A , LFMP B The electrochemical impedance spectroscopy of LFMPs and LFMPs after 500 cycles at 25 °C was used to determine the A , LFMP BThe capacity retention rates of LFMPs after 300 and 500 cycles of charge and discharge at 1C current are shown in Table 7; and the capacity retention rates of LFMPs after 300 and 500 cycles of charge and discharge at 1C current are determined respectively. A LFMP B The resistance fitting values ​​of the cyclic resistance of LFMPs after 300 and 500 charge and discharge cycles at 1C current are shown in Table 8.

[0099] Table 7 LFMP A LFMP B Capacity retention of LFMPs after 300 and 500 cycles at 25°C and 1C

[0100] Cathode Materials Capacity retention after 300 cycles at 25℃ (%) Capacity retention after 500 cycles at 25℃ (%) <![CDATA[LFMP A ]]> 94.77 87.81 <![CDATA[LFMP B ]]> 94.91 90.06 <![CDATA[LFMP S ]]> 95.03 92.21

[0101] Table 8 LFMP A LFMP B The resistance fitting values ​​of the cyclic resistance of LFMPs after 500 cycles at 25℃

[0102]

[0103] The capacity retention rate of three kinds of lithium manganese iron phosphate cathode materials at 1C after cycling was analyzed and compared. After the existing technology was used for charge and discharge cycles, the cycle performance did not fluctuate much in the first 300 cycles, and it was impossible to compare the advantages and disadvantages of the cycle performance of the three cathode materials. During these 300 cycles, the test time required for constant current charging and constant current discharging required 600h (each charge and discharge cycle was calculated as 2h). If the standing time required for each cycle is taken into account, the time required to evaluate the cycle performance of the cathode material will be longer. If it continues to increase to 500 charge and discharge cycles, the time required to evaluate the cycle performance of the cathode material will be further extended, the evaluation time cost is huge, and the loss of the detection instrument and the economic cost of energy loss will also increase.

[0104] The evaluation of the cycle performance of the positive electrode material in this application is only 30 cycles at most, which takes less than 70 hours, greatly reducing the evaluation time and thus significantly reducing the evaluation cost.

[0105] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0106] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for evaluating the cycle performance of lithium manganese iron phosphate positive electrode material, characterized in that: include: Obtain standard positive electrode materials of lithium manganese iron phosphate and positive electrode materials to be tested; Based on the standard positive electrode material and the positive electrode material to be tested, a standard battery and a battery to be tested are prepared according to the same process respectively; The standard battery and the battery to be tested are subjected to activation and constant capacity treatment under the same conditions; The standard battery and the battery to be tested after the activation and constant capacity treatment are charged to a first target voltage respectively, and the electrochemical impedance spectra of the standard battery and the battery to be tested are collected respectively after being placed for a first static time to obtain the corresponding standard sample charging resistance and the sample to be tested charging resistance respectively; The standard battery and the battery to be tested are respectively subjected to charge-discharge cycles at a preset ambient temperature, and electrochemical impedance spectra of the standard battery and the battery to be tested are respectively collected after being placed for a second rest time under multiple preset charge states, to obtain a standard sample cycle resistance corresponding to the preset charge state and a sample cycle resistance corresponding to the preset charge state; The charging resistance of the standard sample and the charging resistance of the sample to be tested, the cycling resistance of the standard sample and the cycling resistance of the sample to be tested are compared respectively, and the cycling performance relationship between the standard positive electrode material of the lithium manganese iron phosphate positive electrode material and the positive electrode material to be tested is determined according to the comparison results.

2. The evaluation method according to claim 1, characterized in that: The standard for judging the cycle performance relationship between the standard positive electrode material of the lithium manganese iron phosphate positive electrode material and the positive electrode material to be tested is: If the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample, and the cycle resistances of the samples to be tested are greater than the cycle resistances of the standard samples, it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is lower than the cycle performance of the standard positive electrode material; If the charging resistance of the sample to be tested is smaller than the charging resistance of the standard sample, and the cycle resistance of each of the samples to be tested is smaller than the cycle resistance of each of the standard samples, it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is higher than the cycle performance of the standard positive electrode material.

3. The evaluation method according to claim 2, characterized in that: The preset state of charge includes a first state of charge, a second state of charge, a third state of charge and a fourth state of charge, the standard sample circulation resistance includes a first standard sample circulation resistance corresponding to the first state of charge, a second standard sample circulation resistance corresponding to the second state of charge, a third standard sample circulation resistance corresponding to the third state of charge, and a fourth standard sample circulation resistance corresponding to the fourth state of charge, and the sample circulation resistance to be tested includes a first sample circulation resistance to be tested corresponding to the first state of charge, a second sample circulation resistance to be tested corresponding to the second state of charge, a third sample circulation resistance to be tested corresponding to the third state of charge, and a fourth sample circulation resistance to be tested corresponding to the fourth state of charge; Among them, the first state of charge<the second state of charge<the third state of charge<the fourth state of charge.

4. The evaluation method according to claim 3, characterized in that: If the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample, and the cycle resistance of each of the samples to be tested is greater than the cycle resistance of each of the standard samples, then it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is lower than the cycle performance of the standard positive electrode material, including: If the charging resistance of the sample to be tested is greater than the charging resistance of the standard sample, the cycling resistance of the first sample to be tested is greater than the cycling resistance of the first standard sample, the cycling resistance of the second sample to be tested is greater than the cycling resistance of the second standard sample, the cycling resistance of the third sample to be tested is greater than the cycling resistance of the third standard sample, and the cycling resistance of the fourth sample to be tested is greater than the cycling resistance of the fourth standard sample, then it is determined that the cycling performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is lower than the cycling performance of the standard positive electrode material.

5. The evaluation method according to claim 3, characterized in that: If the charging resistance of the sample to be tested is smaller than the charging resistance of the standard sample, and the cycle resistances of the samples to be tested are smaller than the cycle resistances of the standard samples, then it is determined that the cycle performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is higher than the cycle performance of the standard positive electrode material, including: If the charging resistance of the sample to be tested is smaller than the charging resistance of the standard sample, the cycling resistance of the first sample to be tested is smaller than the cycling resistance of the first standard sample, the cycling resistance of the second sample to be tested is smaller than the cycling resistance of the second standard sample, the cycling resistance of the third sample to be tested is smaller than the cycling resistance of the third standard sample, and the cycling resistance of the fourth sample to be tested is smaller than the cycling resistance of the fourth standard sample, then it is determined that the cycling performance of the positive electrode material to be tested of the lithium manganese iron phosphate positive electrode material is higher than the cycling performance of the standard positive electrode material.

6. The evaluation method according to claim 3, characterized in that: The first state of charge is 5% to 15%, the second state of charge is 75% to 85%, the third state of charge is 92.5% to 97.5%, and the fourth state of charge is 100%.

7. The evaluation method according to claim 1, characterized in that: The activation and constant volume treatment comprises: The battery to be tested and the standard battery are respectively charged to a second target voltage by constant current and constant voltage, and are placed for a third rest time; Discharging the battery to be tested and the standard battery at a constant current to a third target voltage respectively, and then placing them for a fourth rest time; The activation and constant volume treatment is performed for 1 to 5 cycles; And / or, the second target voltage is 3.7V to 4.2V; And / or, the third target voltage is 1.8V to 2.0V; And / or, the third standing time and the fourth standing time are both 5 min to 30 min; And / or, the constant current and constant voltage charging and the constant current discharging are both performed under the condition of 0.01C to 0.1C.

8. The evaluation method according to claim 1, wherein: The first standing time is 0.5h to 2h, and the second standing time is 1.0h to 5.0h; And / or, the charge-discharge cycle is performed for 10 to 30 cycles under 0.5C to 5C conditions.

9. The evaluation method according to claim 1, characterized in that: The preset ambient temperature is 25°C to 60°C; And / or, the charging to the first target voltage is performed under the condition of 0.01C to 0.1C, and the first target voltage is 3.7V to 4.2V.

10. The evaluation method according to claim 1, wherein: The electrochemical workstation used for collecting electrochemical impedance spectroscopy had a polarization voltage of 10 mV and a frequency of 0.001 Hz to 100,000 Hz.

Citation Information

Cited By

  • Detection method and detection equipment for positive electrode active material

    CN120703588A

  • Cathode material cycle performance prediction method

    CN121049764A