Preparation method of laminated ferrite inductor

Through liquid nitrogen cooling and magnetization treatment combined with magnetic field annealing technology, the temperature resistance stability problem of stacked ferrite inductors is solved, and high-performance temperature resistance stability and low-cost process flow are achieved.

CN118983182APending Publication Date: 2024-11-19GUANGDONG FENGHUA ADVANCED TECHNOLOGY (HOLDING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126679.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

There are problems with the temperature stability of laminated ferrite inductors, and the prior art is difficult to effectively solve the problem of large rate of change in sensing.

Method used

Through the adjustment process, the sintered laminated inductor cooked magnets are cooled at low temperature in liquid nitrogen, magnetized after electroplating, and annealing in a magnetic field to ensure the temperature stability of the magnetic functional grain structural phase.

Benefits of technology

The temperature resistance stability of the laminated ferrite inductor has been significantly improved, and the sensor change rate is reduced from >20% to less than 10%. After 30 days of standing, the sensor change rate is less than 2%, which meets the high temperature resistance change rate. Application requirements, simple and controllable process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983182A_ABST
    Figure CN118983182A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a laminated ferrite inductor, and relates to the technical field of laminated ferrite inductors. The invention discloses a preparation method of a laminated ferrite inductor. The preparation method comprises the following steps: (1) preparing a sintered laminated inductor cooked blank magnet; (2) immersing the sintered laminated inductor cooked blank magnet into liquid nitrogen for cooling treatment to obtain a sintered magnet semi-finished product; (3) chamfering, end sealing, end burning and electroplating are carried out on the sintered magnet semi-finished product to obtain the laminated ferrite inductor, and magnetization treatment is carried out on the electroplated laminated ferrite inductor; and (4) carrying out magnetic field annealing treatment on the product treated in the step (3), taking the product out of the box and cooling the product to room temperature to obtain a laminated ferrite inductor finished product. The method provided by the invention can effectively solve the problem that the temperature-resistant change rate of the sensing value is large in the manufacturing and application of the existing laminated ferrite inductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laminated ferrite inductors, and in particular to a method for preparing the laminated ferrite inductor. Background Art

[0002] Ferrite chip inductors are the mainstream multilayer chip inductors. The magnetic material used in the product structure is NiCuZn ferrite material, which has become an important branch of ferrite materials. It can significantly improve the sintering characteristics of the product matrix, and has adaptive adjustments and improvements to the material's magnetic permeability, power consumption, volume density, magnetic functional grain structure phase, applicable frequency band, etc. The technology is becoming more mature and its application scenarios are constantly expanding.

[0003] Conventional methods to improve the temperature stability of multilayer ferrite inductor products are to modify the original powder material of the matrix, which is to change and improve the temperature characteristics of the product to a certain extent by adjusting the properties such as grain, resistivity, and magnetic permeability. However, the temperature stability of chip inductor components is not solely determined by the temperature stability of the material. In the process of forming the matrix magnetic functional grain structure phase of the product, the powder and slurry are constantly affected by the composite influence of multiple parameter factors such as production preparation, sintering heat treatment process, etc., which will also affect the temperature stability of the final product. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a laminated ferrite inductor. Based on the product process characteristics, the present invention adjusts the technical process defects to ensure that the functional grain structure phase in the product magnet is in a temperature-stable state, thereby solving the problem of temperature stability of the laminated ferrite inductor.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The present invention provides a method for preparing a laminated ferrite inductor, comprising the following steps:

[0007] (1) preparing a sintered laminated inductor green magnet;

[0008] (2) immersing the sintered laminated inductor green body magnet in liquid nitrogen for cooling for 5-10 minutes to obtain a sintered magnet semi-finished product;

[0009] (3) The sintered magnet semi-finished product is then chamfered, sealed, burned, and electroplated to obtain a laminated ferrite inductor, and the electroplated laminated ferrite inductor is then magnetized for 3-10 minutes;

[0010] (4) The product after the treatment in step (3) is then subjected to magnetic field annealing treatment, the annealing temperature is 120-150° C., the magnetic field strength is 5-10 mT, the insulation time is 60-90 min, and the product is taken out of the box and cooled to room temperature to obtain a finished laminated ferrite inductor.

[0011] The present invention controls the magnetic moment coupling characteristics in the grain structure phase of the inductor magnet by immersing the sintered laminated inductor blank magnet in liquid nitrogen for low temperature cooling treatment, and ensures the temperature relative stability of the ferrimagnetic structure phase. Then, magnetization treatment and magnetic field annealing technical process steps are added after the electroplating process, and a composite process step is formed with the liquid nitrogen cooling technical process after the sintered magnet, so that the magnetic functional grain structure phase of the product can reach the best temperature resistance stability state, thereby effectively solving the problem of large temperature resistance change rate of inductance in the existing laminated ferrite inductor during manufacturing and application.

[0012] Preferably, the method for preparing the sintered laminated inductor green magnet in step (1) comprises: preparing slurry, tape casting, printing electrodes, cutting, debinding and sintering, so as to obtain the sintered laminated inductor green magnet.

[0013] Preferably, the slurry is formed by mixing a ferrite material and a casting agent.

[0014] Preferably, the casting agent carrier is a mixture of various organic substances, and the casting agent includes a resin binder, a dispersant, isobutanol, and n-propyl acetate; the added amounts of the resin binder, the dispersant, isobutanol, and n-propyl acetate are 40-45%, 5-10%, 10-20%, and 50-80% of the total weight of the ferrite material and the casting agent, respectively.

[0015] Preferably, the resin adhesive is a phenolic epoxy resin, which has good adhesion to the metal oxide substrate and excellent mechanical properties.

[0016] Preferably, the dispersant is a polyacrylic acid macromolecular polymer, which is a surfactant having two opposite properties, lipophilicity and hydrophilicity, and can rapidly wet the surface of solid particles and raise the energy barrier between solid particles to a sufficiently high level.

[0017] In the present invention, when adding the casting agent carrier, it is added in a proportion based on the mixture of the main component and the additive. This proportion expression is also commonly used in experimental papers related to ferrite materials.

[0018] The process window for the proportion of resin binder, dispersant, isobutanol and n-propyl acetate is relatively wide and has little effect on the performance of the main inorganic component, that is, there is an allowable error in the content ratio. The role of resin binder, dispersant, isobutanol and n-propyl acetate is to shape the material into a uniform membrane. They will volatilize through oxidation reaction after sintering in the sample debinding and sintering stage, leaving very little residue and having almost no effect on material properties.

[0019] Preferably, in step (2), the cooling temperature is -230°C to -180°C, and the cooling time is 6-8 minutes.

[0020] Preferably, the magnetization treatment method in step (3) is as follows: placing the electroplated laminated ferrite inductor in a high-strength external magnetic field of a neodymium iron boron magnet, with a magnetic field strength of 200-400 mT, and leaving it to stand for 3-10 minutes.

[0021] The present invention can only ensure the excellent temperature resistance stability of the laminated ferrite inductor by magnetizing it in a high-intensity external magnetic field. The temperature resistance stability of the response inductor prepared by magnetizing it in a weak magnetic field decreases by more than 5%, which is not conducive to product application.

[0022] Preferably, the magnetization temperature in step (3) is 25-30°C.

[0023] Preferably, the magnetic field annealing in step (4) is performed by combining a constant current source and a copper wire winding coil, the output current of the constant current source is 3-15A, and the number of winding coils is 200-400 turns.

[0024] Preferably, the coil is tightly wound, and the shape of a single winding is a square with a single side length of 0.2-0.4m, and the length of a single-layer winding coil group is not less than 0.5m.

[0025] Preferably, in step (4), the annealing temperature is 130-140° C., the magnetic field strength is 6-8 mT, and the holding time is 70-80 min.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The laminated ferrite inductor prepared by the present invention is subjected to liquid nitrogen cooling after sintering the magnet, magnetization treatment after electroplating, and magnetic field annealing treatment. The temperature resistance stability of the finished product after three reflow soldering is improved, and the inductance change rate is reduced from >20% to less than 10%; the inductance change rate of the finished product after 30 days of static placement is less than 2% and the proportion is ≥90%; the inductance change rate of the finished product after 30 days of static placement is less than 5% and the proportion is 100%, making the defective rate 0, which has obvious advantages over existing similar products and can meet the application requirements with extremely high requirements for temperature resistance change rate. In addition, the method described in the present invention is simple and controllable, low-cost, and can be processed in batches to improve product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the magnetic field coil structure in the magnetic field annealing heat treatment technology process of the present invention. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.

[0030] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0031] The inductors prepared in the embodiments of the present invention are all 2012 size 33uH±10% inductors (length 2mm, width 1.2mm), and the described inductor performances are all the performances of 2012 size inductors. Other technicians in the field can use the invention content of this patent or make limited changes to prepare other sizes of multilayer inductors to achieve similar beneficial effects without creative work, which are all within the protection scope of the present invention application.

[0032] The sintered magnet of the multilayer ferrite inductor prepared in the embodiment of the present invention is manufactured by a general multilayer inductor manufacturing process. The detailed process can be referred to Chapter 7 of the books "Multilayered Low Temperature Cofired Ceramics" and "Design and Application of Soft Ferrite Devices".

[0033] Example 1

[0034] This embodiment discloses a method for preparing a laminated ferrite inductor, comprising the following steps:

[0035] (1) Preparing a sintered laminated inductor green magnet: preparing slurry, tape casting, printing electrodes, cutting, debinding and sintering to obtain a sintered laminated inductor green magnet;

[0036] The slurry is prepared by uniformly mixing the ferrite material and the casting agent carrier: the casting agent includes a resin binder, a dispersant, isobutyl alcohol, and n-propyl acetate; the added amounts of the resin binder, the dispersant, isobutyl alcohol, and n-propyl acetate are 40%, 5%, 10%, and 80% of the total weight of the ferrite material and the casting agent, respectively; the resin binder is a phenolic epoxy resin, and the dispersant is dibutyl phthalate.

[0037] (2) The sintered laminated inductor green body magnet is immersed in liquid nitrogen (-196°C) for low temperature cooling treatment. The liquid nitrogen cooling treatment time is 5 minutes to obtain a sintered magnet semi-finished product.

[0038] (3) The sintered magnet semi-finished product is then chamfered, capped, sintered, and electroplated to obtain a laminated ferrite inductor, which is then further processed. The electroplated laminated ferrite inductor is placed in a high-intensity external magnetic field of a neodymium iron boron magnet at room temperature of 25° C. for magnetization treatment, and the magnetization time is 5 minutes.

[0039] (4) The product treated in step (3) is then placed in a magnetic field coil inside a coil device in an oven for magnetic field annealing, the annealing temperature is 130° C., the magnetic field intensity is 8 mT, the insulation time is 80 min, and then taken out of the box and cooled to room temperature. Finally, after inspection and taping, a finished laminated ferrite inductor is obtained.

[0040] Example 2

[0041] This embodiment discloses a method for preparing a laminated ferrite inductor, comprising the following steps:

[0042] (1) Preparing a sintered laminated inductor green magnet: preparing slurry, tape casting, printing electrodes, cutting, debinding and sintering to obtain a sintered laminated inductor green magnet;

[0043] The slurry is prepared by uniformly mixing the ferrite material and the casting agent carrier: the casting agent includes a resin binder, a dispersant, isobutyl alcohol, and n-propyl acetate; the added amounts of the resin binder, the dispersant, isobutyl alcohol, and n-propyl acetate are 45%, 10%, 20%, and 50% of the total weight of the ferrite material and the casting agent, respectively; the resin binder is a phenolic epoxy resin, and the dispersant is a polyacrylic acid high molecular polymer.

[0044] (2) The sintered laminated inductor green body magnet is immersed in liquid nitrogen for low-temperature cooling treatment. The liquid nitrogen cooling treatment time is 3 minutes to obtain a sintered magnet semi-finished product.

[0045] (3) The sintered magnet semi-finished product is then chamfered, capped, sintered, and electroplated to obtain a laminated ferrite inductor, which is then further processed. The electroplated laminated ferrite inductor is placed in a high-intensity external magnetic field of a neodymium iron boron magnet at room temperature of 25° C. for magnetization treatment, and the magnetization time is 3 minutes.

[0046] (4) The product treated in step (3) is then placed in a magnetic field coil inside a coil device in an oven for magnetic field annealing, the annealing temperature is 120° C., the magnetic field intensity is 5 mT, the insulation time is 60 min, and then taken out of the box and cooled to room temperature. Finally, after inspection and taping, a finished laminated ferrite inductor is obtained.

[0047] Example 3

[0048] This embodiment discloses a method for preparing a laminated ferrite inductor, comprising the following steps:

[0049] (1) Preparing a sintered laminated inductor green magnet: preparing slurry, tape casting, printing electrodes, cutting, debinding and sintering to obtain a sintered laminated inductor green magnet;

[0050] The slurry is prepared by uniformly mixing the ferrite material and the casting agent carrier: the casting agent includes a resin binder, a dispersant, isobutyl alcohol, and n-propyl acetate; the added amounts of the resin binder, the dispersant, isobutyl alcohol, and n-propyl acetate are 43%, 8%, 12%, and 70% of the total weight of the ferrite material and the casting agent, respectively; the resin binder is a phenolic epoxy resin, and the dispersant is butyl benzyl phthalate.

[0051] (2) The sintered laminated inductor green body magnet is immersed in liquid nitrogen for low-temperature cooling treatment. The liquid nitrogen cooling treatment time is 10 minutes to obtain a sintered magnet semi-finished product.

[0052] (3) The sintered magnet semi-finished product is then chamfered, sealed, sintered, and electroplated to obtain a laminated ferrite inductor, which is then further processed. The electroplated laminated ferrite inductor is placed in a high-intensity external magnetic field of a neodymium iron boron magnet at room temperature of 25° C. for magnetization treatment, and the magnetization time is 10 minutes.

[0053] (4) The product treated in step (3) is then placed in a magnetic field coil inside a coil device in an oven for magnetic field annealing, the annealing temperature is 150° C., the magnetic field intensity is 8 mT, the insulation time is 90 min, and then taken out of the box and cooled to room temperature. Finally, after inspection and taping, a finished laminated ferrite inductor is obtained.

[0054] Comparative Example 1

[0055] A method for preparing a laminated ferrite inductor is different from that of Example 1 in that the sintered laminated inductor is not subjected to magnetization and magnetic field annealing treatment, and the other steps are the same as those of Example 1.

[0056] Comparative Example 2

[0057] A method for preparing a laminated ferrite inductor is different from that of Example 1 in that the sintered laminated inductor is not subjected to liquid nitrogen treatment, magnetization and magnetic field annealing treatment, and the other steps are the same as those of Example 1.

[0058] Comparative Example 3

[0059] A method for preparing a laminated ferrite inductor is different from that of Example 1 in that the sintered laminated inductor is not subjected to liquid nitrogen treatment and magnetization treatment, and the other steps are the same as those of Example 1.

[0060] Comparative Example 4

[0061] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the liquid nitrogen treatment time in step (2) is 1 minute, and the other steps are the same as Example 1.

[0062] Comparative Example 5

[0063] A method for preparing a laminated ferrite inductor, which is different from that of Example 1 in that the liquid nitrogen treatment time in step (2) is 15 minutes, and the other steps are the same as those of Example 1.

[0064] Comparative Example 6

[0065] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the magnetization time in step (3) is 1 minute, and the other steps are the same as Example 1.

[0066] Comparative Example 7

[0067] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the magnetization time in step (3) is 15 minutes, and the other steps are the same as Example 1.

[0068] Comparative Example 8

[0069] A method for preparing a laminated ferrite inductor, which is different from that of Example 1 in that the annealing temperature in step (4) is 60° C., and the other steps are the same as those of Example 1.

[0070] Comparative Example 9

[0071] A method for preparing a laminated ferrite inductor, which is different from that of Example 1 in that the annealing temperature in step (4) is 200° C., and the other steps are the same as those of Example 1.

[0072] Comparative Example 10

[0073] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the magnetic field intensity in step (4) is 2mT, and the other steps are the same as Example 1.

[0074] Comparative Example 11

[0075] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the magnetic field strength in step (4) is 15 mT, and the other steps are the same as Example 1.

[0076] Comparative Example 12

[0077] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the holding time in step (4) is 20 minutes, and the other steps are the same as Example 1.

[0078] Comparative Example 13

[0079] A method for preparing a laminated ferrite inductor, which is different from Example 1 in that the holding time in step (4) is 200 minutes, and the other steps are the same as Example 1.

[0080] Performance Testing

[0081] The inductance value is detected using the test instrument Keysight E4982A, the fixture Keysight 16192A, the test frequency is 1MHz, and the test signal condition is 50mV.

[0082] Sensitivity temperature resistance 3 times reflow soldering change rate (△L 3T ) The detection method is: Use the above E4982A test instrument to test the inductance value (L0) of 50-100 finished inductors before reflow soldering and the inductance value (L1) after 3 reflow soldering, and use the formula △L 3T =(L1-L0) / L0*100%, and the product performance is evaluated by the maximum value of the change rate; the 3-time reflow treatment method is to place the sample on a plastic carrier, pass through the reflow oven and then cool to room temperature, and cycle 3 times. The highest temperature zone of the reflow oven is set at 265℃±5℃, the speed of the reflow oven conveyor is 50-80cm / min, and the sample in and out cycle is 9-12min.

[0083] 30-day sensitivity change rate (△L 30 ) The detection method is: Use the above E4982A test instrument to test the inductance value (L0) of 50-100 finished inductors before placement and the inductance value (L2) after placement for 30 days, and use the formula △L 30 =(L2-L0) / L0*100% calculated; the placement method is to place the sample on a plastic carrier plate, and to prevent external interference, the sample plate is placed in an anti-magnetic sample box and left to stand for 30 days.

[0084] The above test results are shown in Table 1.

[0085] Table 1

[0086]

[0087]

[0088] It can be seen from Example 1 that the sintered magnet is cooled with liquid nitrogen for 5 minutes, and the magnetization treatment process is carried out in a high-intensity external magnetic field of the NdFeB magnet for 5 minutes, and then a composite magnetic field annealing process is further performed. The magnetic field annealing oven temperature is 130°C, the magnetic field intensity in the magnetic field annealing coil is 8mT, and the magnetic field annealing holding time is 80min. The obtained inductor sample is tested for reliability, showing that the inductance meets the standard of 33uH±10%, the temperature resistance change rate of 3 reflow soldering is ≤4.06%, the proportion of inductance change rate of <2% after 30 days is ≥90%, and the proportion of inductance change rate of <5% after 30 days is 100%, and the inductance performance is excellent.

[0089] Compared with Example 1, in the composite process parameter range applicable to the present invention, the liquid nitrogen treatment time of the sintered magnet is first reduced to 3 minutes, the magnetization treatment time is then reduced to 3 minutes, the temperature of the magnetic field annealing oven is reduced to 120°C, the magnetic field strength in the coil is reduced to 5mT, and the magnetic field annealing holding time is reduced to 60 minutes. The obtained inductor sample has been tested for reliability, and its various performance test values ​​are excellent. The inductor sample shows that the inductance reaches the standard of 33uH±10%, the temperature resistance 3 times reflow soldering change rate is ≤9.22%, the proportion of inductance change rate of <2% after 30 days is ≥90%, and the proportion of inductance change rate of <5% after 30 days is 100%.

[0090] Example 3 Compared with Example 1, within the composite process parameter range applicable to the present invention, the liquid nitrogen treatment time of the sintered magnet is first increased to 10 minutes, and then the magnetization treatment time is increased to 10 minutes, the temperature of the magnetic field annealing oven is increased to 150°C, the magnetic field strength in the coil is increased to 8mT, and the magnetic field annealing holding time is increased to 90 minutes. The obtained inductor sample has been tested for reliability, and its various performance test values ​​are excellent. The inductor sample shows that the inductance meets the standard of 33uH±10%, the temperature resistance 3 times reflow soldering change rate is ≤6.10%, the proportion of inductance change rate of <2% after 30 days is ≥90%, and the proportion of inductance change rate of <5% after 30 days is 100%.

[0091] Comparative Example 1 is a conventional production process. Compared with Example 1, only liquid nitrogen treatment time is 5min, no magnetization treatment is performed, and no magnetic field annealing technology process treatment is performed. The obtained inductor sample is tested for reliability, showing that the inductance meets the standard of 33uH±10%, but the inductance temperature resistance 3 times reflow soldering change rate is ≥20%, the proportion of inductance change rate <2% after 30 days of placement is ≤60%, and the proportion of inductance change rate <5% after 30 days of placement is ≤80%, which is worse than the performance of the sample in Example 1.

[0092] Comparative Example 2 and Comparative Example 3 do not use liquid nitrogen treatment or magnetization treatment. In the subsequent process, Comparative Example 2 does not use the magnetic field annealing technology, and Comparative Example 3 uses the same magnetic field annealing process as Example 1. After reliability testing, the obtained inductor samples showed an inductance of <33uH±10%, and the inductance did not meet the standard. The inductance change rate after 3 times of reflow soldering was ≥15% and ≤9.74% respectively. The proportion of inductance change rate <2% after 30 days of placement was ≤50%, and the proportion of inductance change rate <5% after 30 days of placement was ≤70% and ≤60% respectively. The product inductance was unqualified and the overall performance was poor.

[0093] Compared with Example 1, Comparative Example 4 only changes the liquid nitrogen cooling time in the composite process to 1 minute. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of temperature resistance for 3 reflow soldering is ≥10%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%, which is worse than the performance of the sample in Example 1.

[0094] Compared with Example 1, Comparative Example 5 only changes the liquid nitrogen cooling time in the composite process to 15min. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of temperature resistance for 3 times of reflow soldering is ≤5.28%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%. Compared with Example 1, its liquid nitrogen treatment time is long and the process cost is high.

[0095] Compared with Example 1, Comparative Example 6 only changes the magnetization treatment time in the composite process to 1 minute. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the temperature resistance 3 times reflow soldering change rate is ≥10%, the proportion of inductance change rate of <2% after 30 days placement is ≥90%, and the proportion of inductance change rate of <5% after 30 days placement is 100%, which is worse than the performance of the sample in Example 1.

[0096] Compared with Example 1, Comparative Example 7 only changes the magnetization treatment time in the composite process to 15min. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of heat resistance for 3 times of reflow soldering is ≤5.11%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%. Compared with Example 1, its magnetization treatment time is long and the process cost is high.

[0097] Compared with Example 1, Comparative Example 8 only changes the temperature of the magnetic field annealing oven in the composite process to 60°C. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of temperature resistance for 3 reflow soldering is ≥10%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%, which is worse than the performance of the sample in Example 1.

[0098] Compared with Example 1, Comparative Example 9 only changes the temperature of the magnetic field annealing oven in the composite process to 200°C. After reliability testing, the obtained inductor samples show that the inductance meets the standard of 33uH±10%, the change rate of temperature resistance for 3 times of reflow soldering is ≤4.29%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%. Compared with Example 1, the magnetic field annealing oven temperature is as high as 200°C, which has a deteriorating effect on the silver electrode at the end of the product, and there is a risk of causing the appearance of the silver electrode at the end to turn black and affect the product quality. In addition, the high temperature will cause high energy consumption of the equipment and high process cost.

[0099] Compared with Example 1, Comparative Example 10 only changes the magnetic field strength in the coil in the composite process to 2mT. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of temperature resistance for 3 reflow soldering is ≥10%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%, which is worse than the performance of the sample in Example 1.

[0100] Compared with Example 1, Comparative Example 11 only changes the magnetic field strength in the coil in the composite process to 15mT. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the temperature resistance 3 times reflow soldering change rate is ≤6.08%, the proportion of inductance change rate of <2% after 30 days of placement accounts for ≥90%, and the proportion of inductance change rate of <5% after 30 days of placement accounts for 100%. The performance is worse than that of the sample in Example 1, and the equipment consumes high energy and the process cost is high.

[0101] Compared with Example 1, Comparative Example 12 only changes the magnetic field annealing holding time in the composite process to 20 minutes. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of heat resistance for 3 times of reflow soldering is ≥10%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%, which is worse than the performance of the sample in Example 1.

[0102] Compared with Example 1, Comparative Example 13 only changes the magnetic field annealing holding time in the composite process to 200min. The obtained inductor samples are tested for reliability, showing that the inductance reaches the standard of 33uH±10%, the change rate of heat resistance for 3 times of reflow soldering is ≤5.51%, the proportion of inductance change rate after 30 days of placement <2% accounts for ≥90%, and the proportion of inductance change rate after 30 days of placement <5% accounts for 100%. Compared with Example 1, its magnetic field annealing holding time is long and the process cost is high.

[0103] In general, the composite process preparation method of the present invention can effectively obtain a high-performance laminated ferrite inductor with inductance meeting the range standard, a small change rate of temperature resistance after three reflow soldering, that is, high temperature resistance stability, good stability after being placed for 30 days, and low process cost. Liquid nitrogen cooling of the sintered magnet can enhance the microscopic magnetic moment coupling strength of the magnet, and magnetization treatment after electroplating can further enhance the magnetic moment coupling effect. Combined with the magnetic field annealing technology process, the inductance value can be close to the optimal magnetic domain stability state, thereby ensuring the temperature resistance stability of the inductor.

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a laminated ferrite inductor, characterized in that: The following steps are involved: (1) preparing a sintered laminated inductor green magnet; (2) immersing the sintered laminated inductor green body magnet in liquid nitrogen for cooling for 5-10 minutes to obtain a sintered magnet semi-finished product; (3) The sintered magnet semi-finished product is then chamfered, sealed, burned, and electroplated to obtain a laminated ferrite inductor, and the electroplated laminated ferrite inductor is then magnetized for 3-10 minutes; (4) The product after the treatment in step (3) is then subjected to magnetic field annealing treatment, the annealing temperature is 120-150° C., the magnetic field strength is 5-10 mT, the insulation time is 60-90 min, and the product is taken out of the box and cooled to room temperature to obtain a finished laminated ferrite inductor.

2. The method for preparing a laminated ferrite inductor according to claim 1, wherein: The method for preparing the sintered laminated inductor green magnet in the step (1) comprises: preparing slurry, tape casting, printing electrodes, cutting, debinding and sintering, so as to obtain the sintered laminated inductor green magnet.

3. The method for preparing a laminated ferrite inductor according to claim 2, wherein: The slurry is prepared by mixing a ferrite material and a casting agent.

4. The method for preparing a laminated ferrite inductor according to claim 3, wherein: The casting agent comprises a resin binder, a dispersant, isobutyl alcohol and n-propyl acetate.

5. The method for preparing a laminated ferrite inductor according to claim 4, wherein: The added amounts of the resin binder, dispersant, isobutyl alcohol and n-propyl acetate are 40-45%, 5-10%, 10-20% and 50-80% of the total weight of the ferrite material and the casting agent respectively.

6. The method for preparing a laminated ferrite inductor according to claim 5, wherein: The resin adhesive is a phenolic epoxy resin; the dispersant is a polyacrylic acid macromolecular polymer.

7. The method for preparing a laminated ferrite inductor according to claim 1, wherein: The magnetization treatment method in step (3) is specifically as follows: placing the electroplated laminated ferrite inductor in a high-intensity external magnetic field of a neodymium iron boron magnet and leaving it to stand for 3-10 minutes.

8. The method for preparing a laminated ferrite inductor according to claim 1, wherein: In the step (4), the magnetic field annealing is performed by combining a constant current source and a copper wire winding coil, the output current of the constant current source is 3-15A, and the number of winding coils is 200-400 turns.

9. The method for preparing a laminated ferrite inductor according to claim 8, wherein: The shape of the single winding coil is a square with a single side length of 0.2-0.4 m, and the length of the single-layer winding coil group is not less than 0.5 m.

10. The method for preparing a laminated ferrite inductor according to claim 1, wherein: In the step (4), the annealing temperature is 130-140° C., the magnetic field strength is 6-8 mT, and the insulation time is 70-80 min.