Method of forming gate stack of multi-gate device and transistor
By forming an in-situ fluorine-free tungsten layer above the silicon-containing cap layer in a multi-gate device and configuring a work function layer with low aluminum content, the problems of increasing gate resistance and oxidation effects are solved, and the device speed and performance are improved.
Patent Information
- Application Number
- CN202410991155.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-30
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-19
AI Technical Summary
In multi-gate devices, the manufacturing of gate stacks becomes challenging as the IC technology nodes shrink, especially under reduced size conditions, the gate resistance increases, which is susceptible to oxidation, resulting in performance degradation. Such as device speed slowing and threshold voltage changes.
By forming an in-situ fluorine-free tungsten layer above the silicon-containing cap layer without breaking the vacuum, and forming a fluorine-free tungsten layer by co-flowing the tungsten precursor and the hydrogen-containing precursor, the gate resistance is reduced and the cap is reduced by reducing the cap. The oxidation and silicon loss of the layer are arranged with a low aluminum content work function layer to further reduce the resistance.
Reducing gate resistance, increasing device speed, reducing threshold voltage variations, and enhancing device performance, especially in ring oscillator applications.
Smart Images

Figure CN118983222A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to methods of forming gate stacks of multi-gate devices and transistors. Background Art
[0002] Multi-gate devices were introduced to meet the growing demand of the semiconductor integrated circuit (IC) industry for smaller and faster electronic devices that can simultaneously support more increasingly complex and sophisticated functions. Multi-gate devices have a gate that extends partially or completely around a channel region to provide access to the channel region on at least two sides. Exemplary multi-gate devices include fin field effect transistors (FinFETs), gate-all-around (GAA) transistors (e.g., nanostructure-based (e.g., nanowire, nanosheet, or nanorod) transistors), other three-dimensional (3D) transistors (e.g., fork-sheet transistors), or combinations thereof. Multi-gate devices enable aggressive scaling of IC technology and have been observed to improve gate control, increase gate-channel coupling, reduce off-state current, and reduce short channel effects (SCEs), while seamlessly integrating with conventional IC manufacturing processes.
[0003] However, as IC technology nodes continue to expand, it becomes challenging to manufacture gate stacks around the channel region of multi-gate devices. For example, the gate stack of a multi-gate device is typically formed using a gate replacement process that includes removing a dummy gate to form a gate opening that exposes a channel layer and filling the gate opening with various gate layers (e.g., a gate dielectric and a gate electrode). The reduction in the size of device components leads to a reduction in the size of the gate opening, which leads to a reduction in the volume of the gate stack. As a result, the gate layer that wraps the channel layer can easily fill the gate opening and / or the space between adjacent channel layers, which leaves limited space in the gate opening for fine-tuning the threshold voltage (Vt) of the multi-gate device, such as by using multiple work function layers and / or thicker work function layers. Various combinations and / or configurations of layers have been explored in the gate stack to maximize the performance of the multi-gate device while minimizing the performance mismatch (such as threshold voltage variation (σVt)) between multi-gate devices of the IC (e.g., those forming memory). While existing gate stack configurations for multi-gate devices and methods of fabricating the same are generally adequate for their intended purposes, they are not completely satisfactory in all respects. Summary of the invention
[0004] According to one aspect of an embodiment of the present application, a method for forming a gate stack of a multi-gate device is provided, the method comprising: forming a gate dielectric above a channel layer; and forming a gate electrode above the gate dielectric by the following steps: forming a work function layer on the gate dielectric, forming a cap above the work function layer, wherein forming the cap comprises forming a metal nitride layer above the work function layer and forming a silicon-containing layer above the metal nitride layer, and forming a fluorine-free tungsten layer above the silicon-containing layer of the cap without breaking the vacuum, wherein forming the fluorine-free tungsten layer above the silicon-containing layer comprises co-flowing a tungsten-containing precursor and a hydrogen-containing precursor.
[0005] According to another aspect of an embodiment of the present application, a method for forming a gate stack of a multi-gate device is provided, the method comprising: forming an interface layer above a first channel layer and a second channel layer, wherein the first channel layer is disposed above the second channel layer; forming a high-k dielectric layer above the interface layer; forming a titanium aluminum carbide layer above the high-k dielectric layer; forming a titanium nitride layer above the titanium aluminum carbide layer; forming a silicon layer above the titanium nitride layer; and co-flowing WCl5 and H2 into a process chamber to form an in-situ fluorine-free tungsten layer above the silicon layer.
[0006] According to another aspect of an embodiment of the present application, a transistor is provided, comprising: a first channel layer and a second channel layer; a gate dielectric surrounding the first channel layer and the second channel layer, wherein the gate dielectric comprises an interface layer and a high-k dielectric layer; and a gate electrode disposed above the gate dielectric, wherein the gate electrode surrounds the first channel layer and the second channel layer, wherein the gate electrode comprises: a titanium aluminum carbide layer disposed above the high-k dielectric layer and a cap disposed above the titanium aluminum carbide layer, wherein the cap comprises a metal nitride layer disposed above the titanium aluminum carbide layer and a silicon layer disposed above the metal nitride layer, and a fluorine-free tungsten layer directly located on the silicon layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Various aspects of the present disclosure can be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be emphasized that, in accordance with standard practice in the industry, the various components are not drawn to scale and are only used for illustrative purposes. In fact, the size of the various components may be arbitrarily increased or reduced for clarity of discussion.
[0008] Figure 1 is a flow chart of a method for fabricating a gate stack of a portion or the entire device according to various aspects of the present disclosure.
[0009] Figure 2 In accordance with various aspects of the present disclosure, a method (such as a gate stack) of a device (such as a transistor) is provided. Figure 1 A partial or overall perspective view of a manufacturing stage associated with a method).
[0010] Figure 3A – Fig.13A and Figure 3B – Fig. 13B In accordance with various aspects of the present disclosure, a method (such as a gate stack) of a device (such as a transistor) is provided. Figure 1 A partial or overall cross-sectional view of each manufacturing stage associated with the method).
[0011] Fig.14A and Fig. 14B Forming a fluorine-free tungsten layer partially or entirely over a silicon layer in accordance with various aspects of the present disclosure is described.
[0012] Fig.15A and Fig. 15B Forming a fluorine-free tungsten layer partially or entirely over a silicon layer according to various aspects of the present disclosure is described.
[0013] Fig.16A and Fig. 16B According to various aspects of the present disclosure, Figure 1 A partial or entire cross-sectional view of a device (such as a transistor) having a gate stack manufactured by the method.
[0014] Fig.17A and Fig. 17B According to various aspects of the present disclosure, Figure 1 A partial or entire cross-sectional view of a device (such as a transistor) having a gate stack manufactured by the method.
[0015] Fig.18A – Fig. 20A and Fig.18B – Fig. 20B According to various aspects of the present disclosure, Figure 1 A partial or whole cross-sectional view of a device (such as a transistor) at various manufacturing stages associated with the method.
[0016] Fig.21 Example circuit schematics showing a portion or the entirety of an inverter according to various aspects of the present disclosure are shown. DETAILED DESCRIPTION
[0017] The present disclosure relates generally to integrated circuit (IC) devices and, more particularly, to gate stacks of transistors and methods of fabricating the same.
[0018] The following disclosure provides many different embodiments or examples for realizing different features of the present invention. The following describes specific examples of components and arrangements to simplify the present disclosure. Of course, these are merely examples and are not restrictive. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component is not directly in contact with the first component. In addition, spatially relative terms, such as, "lower", "upper", "horizontal", "vertical", "above", "above", "below", "below", "upward", "downward", "top", "bottom", etc., and their derivatives (such as "horizontally", "downwardly", "upwardly", etc.) are used to simplify the relationship between one component of the present disclosure and another component. Spatially relative terms are intended to cover different orientations of devices including components. The present disclosure may also repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself specify the relationship between the various embodiments and / or configurations discussed.
[0019] In addition, when a number or a range of numbers is described using the term "about," "approximately," or the like, the term is intended to encompass numbers within a reasonable range that takes into account variations inherent in the manufacturing process as understood by those of ordinary skill in the art. For example, based on known manufacturing tolerances associated with manufacturing features having characteristics associated with the number, the number or range of numbers includes a reasonable range (including the described number), such as within + / -10% of the described number. For example, a material layer having a thickness of "about 5 nm" may encompass a size range of 4.5 nm to 5.5 nm, where the manufacturing tolerance associated with the deposited material layer is + / -10% known to those of ordinary skill in the art. In addition, taking into account the differences inherent in any manufacturing process, when a device component is described as having a "basic" property and / or feature, such terminology is intended to encompass properties and / or features within the tolerance range of the manufacturing process. For example, a "substantially vertical" or "substantially horizontal" feature is intended to encompass features that are approximately vertical and horizontal within a given tolerance range of the manufacturing process used to manufacture such features, but not mathematically or completely vertical and horizontal.
[0020] Multi-gate devices, such as fin field effect transistors (FinFETs), gate-all-around (GAA) transistors, fork-sheet transistors, and other non-planar transistors, have gained popularity due to their enhanced performance compared to traditional planar transistors. As multi-gate device dimensions shrink to facilitate further IC technology node scaling, traditional multi-gate device manufacturing methods face challenges. For example, in gate replacement processes, scaling device dimensions reduces the volume of the gate opening used to fill the gate stack, which reduces the flexibility of gate stack engineering. In addition, the reduced-size gate stack can exhibit a higher total gate resistance (R g ) and are more susceptible to unintentional and / or undesired oxidation of the gate stack, which may result in performance degradation, such as slower device speed and / or undesired threshold voltage (V t ) changes. This problem is exacerbated for some IC applications, such as in ring oscillator (RO) circuits.
[0021] To address these challenges, the present disclosure proposes a gate stack and a method for manufacturing the same that reduces gate resistance. For example, the proposed method for manufacturing a gate stack includes forming a fluorine-free tungsten layer (i.e., an in-situ fluorine-free tungsten layer) above a silicon-containing capping layer without breaking vacuum. This process inhibits oxidation of the silicon-containing capping layer, which improves the deposition / growth of the fluorine-free tungsten layer above the silicon-containing capping layer. In addition, in order to reduce the loss of the silicon-containing capping layer during the deposition / growth of the fluorine-free tungsten layer, a fluorine-free tungsten layer can be formed by co-flowing a tungsten-containing precursor (e.g., WCl5) and a hydrogen-containing precursor (e.g., H2), which reduces the surface reaction of the tungsten-containing precursor with the silicon-containing capping layer. Configuring a gate stack with an in-situ fluorine-free tungsten layer can reduce the gate resistance attributed to the top of the gate stack (e.g., the top disposed above the channel layer of a multi-gate device). In some embodiments, the proposed method for manufacturing a gate stack includes forming a low aluminum content work function layer (e.g., having an aluminum content of less than about 30 atomic %), wherein a silicon-containing capping layer and an in-situ fluorine-free tungsten layer are formed above the low aluminum content work function layer. Reducing the atomic concentration of aluminum in the work function layer can reduce the gate resistance attributed to the inner portion of the gate stack (e.g., the portion disposed between the channel layers of the multi-gate device). Therefore, the gate stack disclosed herein exhibits a lower gate resistance, which can improve device performance, for example, by providing faster device speeds, particularly for IC applications, such as when implemented in a ring oscillator. Details of the improved gate stack for a multi-gate device and methods of manufacturing and / or designing the same are described below. Different embodiments may have different advantages, and any embodiment does not require a particular advantage.
[0022] Figure 1 is a flow chart of a method 100 for partially or entirely fabricating a gate stack of a device according to various aspects of the present disclosure. Figure 2In accordance with various aspects of the present disclosure, a method of manufacturing a gate stack of a device (eg, Figure 1 1. A perspective view of a portion or all of a device 200 at a manufacturing stage associated with method 100). FIG. 3A to FIG. 13A and FIG. 3B to FIG. 13B According to various aspects of the present disclosure, Figure 1 A cross-sectional view of a portion or the entirety of a device 200 at various manufacturing stages associated with the method 100 . Figure 3A and Figure 3B Along Figure 2 A cross-sectional view of the device 200 taken along line AA and line BB, FIG. 4A to FIG. 13A is Figure 1 The subsequent manufacturing stages of method 100 are as follows Figure 2 A cross-sectional view of the device 200 taken along line AA, FIG. 4B to FIG. 13B is Figure 1 The subsequent manufacturing stages of method 100 are along the Figure 2 2 is a cross-sectional view of the device 200 taken along line BB. Fig.14A and Fig. 14B as well as Fig.15A and Fig. 15B Different methods of forming a fluorine-free tungsten layer of a portion or the entire gate stack according to various aspects of the present disclosure are depicted, which may be implemented when fabricating the gate stack of the device 200 . Fig.16A and Fig. 16B According to various aspects of the present disclosure, Figure 1 2 is a cross-sectional view of a device 200 having gate stacks with different configurations manufactured by the method. Fig.17A and Fig. 17B According to various aspects of the present disclosure, Figure 1 FIG. 2 is a cross-sectional view of a device 200 having yet another different configuration of a gate stack fabricated by a method of FIG. Fig.18A – Fig. 20A and Fig.18B – Fig. 20B According to various aspects of the present disclosure Figure 1 A cross-sectional view of a portion or the entirety of a device 200 having another configuration of a gate stack at various stages of the manufacturing process of the method. For ease of description and understanding, this article also discusses Figure 1 , Figure 2 , Figure 3A – Fig.13A , Figure 3B – Fig. 13B , Fig.14A , Fig. 14B , Fig.15A , Fig. 15B , Fig.16A , Fig. 16B , Fig.17A , Fig. 17B , Fig.18A– Fig. 20A and Fig.18B – Fig. 20B . Simplified for clarity Figure 1 , Figure 2 , Figure 3A – Fig.13A , Figure 3B – Fig. 13B , Fig.14A , Fig. 14B , Fig.15A , Fig. 15B , Fig.16A , Fig. 16B , Fig.17A , Fig. 17B , Fig.18A – Fig. 20A and Fig.18B – Fig. 20B , to better understand the inventive concepts of the present disclosure. Figure 1 Additional steps are provided before, during, and after the method 100, and for Figure 1 Additional embodiments of method 100 may move, replace, or eliminate some of the steps described. Additional components may be added to device 200, and some of the components described below may be replaced, modified, or eliminated in other embodiments of device 200.
[0023] Go to Figure 1 , Figure 2 , Figure 3A and Figure 3B , method 100 includes, at box 105, forming a gate structure above the channel layer. The gate structure includes a dummy gate and a gate spacer. This may include receiving and / or forming a device precursor, which includes a substrate (wafer) 202, a semiconductor stack 210 (depicted as having a mesa 202' (i.e., a patterned protruding portion of the substrate 202), a semiconductor layer 215, and a semiconductor layer 220), a substrate isolation structure 222, an internal spacer 224, a source / drain 225, a gate structure 230 (depicted as having a dummy gate 232 and a gate spacer 240), and a dielectric layer 250. The semiconductor stack 210 is in the channel region C of the device 200, and the source / drain 225 is in the source / drain region S / D of the device 200. At Figure 3A In the XZ cross-sectional view, the semiconductor layer 220 and the mesa 202' extend between the source / drain 225 along the X direction, the internal spacer 224 is between the semiconductor layer 215 and the source / drain 225, and the gate structure 230 is disposed above the top of the semiconductor stack 210 and between the source / drain 225. Figure 3B In the embodiment of the present invention (eg, a YZ cross-sectional view), the gate structure 230 is on the top and side of the semiconductor stack 210 , and the gate structure 230 wraps the semiconductor stack 210 .
[0024] The substrate 202 includes: an elemental semiconductor such as silicon and / or germanium; a compound semiconductor such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, indium antimonide, or a combination thereof; an alloy semiconductor such as SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, GaInAsP, or a combination thereof; or a combination thereof. In the depicted embodiment, the substrate 202 is a silicon substrate. In some embodiments, the substrate 202 is a semiconductor-on-insulator substrate such as a silicon-on-insulator (SOI) substrate, a silicon-germanium-on-insulator (SGOI) substrate, or a germanium-on-insulator (GOI) substrate. The substrate 202 (and the mesa 202') may include various doped regions, such as a p-type doped region (e.g., a p-well), an n-type doped region (e.g., an n-well), or a combination thereof. The N-type doped region includes an n-type dopant such as phosphorus, arsenic, other n-type dopants, or a combination thereof. The P-type doped region includes a p-type dopant such as boron, indium, other p-type dopants, or a combination thereof. In some embodiments, the doped region includes a combination of a p-type dopant and an n-type dopant. The doped region can be formed directly on and / or in the substrate 202, for example, to provide a p-well structure, an n-well structure, a double-well structure, a raised structure, other suitable structures, or combinations thereof. In some embodiments, the substrate 202, the mesa 202', and the semiconductor layers thereon include an n-well, for example, when the device 200 is a p-type transistor; or include a p-well, for example, when the device 200 is an n-type transistor.
[0025] The semiconductor stack 210 extends along the x-direction, having a length along the x-direction, a width along the y-direction, and a height along the z-direction. The semiconductor layer 215 and the semiconductor layer 220 are vertically stacked (e.g., along the z-direction) from the top surface of the substrate 202 in a staggered and / or alternating configuration. The composition of the semiconductor layer 215 is different from the composition of the semiconductor layer 220 to achieve etching selectivity and / or different oxidation rates during subsequent processing. For example, the semiconductor layer 215 and the semiconductor layer 220 include different materials, composition atomic percentages, composition weight percentages, thicknesses, or combinations thereof to achieve desired etching selectivity during an etching process (e.g., an etching process implemented to form a suspended channel layer in the channel region C). In some embodiments, the semiconductor layer 215 includes silicon germanium, the semiconductor layer 220 includes silicon, and for a given etchant, the silicon etching rate of the semiconductor layer 220 is different from the silicon germanium etching rate of the semiconductor layer 215. In some embodiments, the semiconductor layer 215 and the semiconductor layer 220 include the same material but different composition atomic percentages to achieve etching selectivity. For example, semiconductor layer 215 and semiconductor layer 220 include silicon germanium with different silicon atomic percentages and / or different germanium atomic percentages. The present disclosure contemplates semiconductor layer 215 and semiconductor layer 220 having any combination of semiconductor materials that provide a desired etch selectivity, a desired oxidation rate difference, a desired performance characteristic (e.g., a material that maximizes current flow), or a combination thereof, including any semiconductor material disclosed herein.
[0026] The substrate isolation structure 222 electrically isolates the active device area and / or the passive device area of the device 200 from each other. For example, the substrate isolation structure 222 separates and electrically isolates the active area of the device 200 (e.g., the semiconductor stack 210 and / or its source / drain 225) from other device areas and / or devices. The substrate isolation structure 222 includes silicon oxide, silicon nitride, silicon oxynitride, other suitable isolation materials (including, for example, silicon, oxygen, nitrogen, carbon, other suitable isolation components, etc.) or a combination thereof. The substrate isolation structure 222 may have a multilayer structure. For example, the substrate isolation structure 222 may include a bulk dielectric (e.g., an oxide layer) on a dielectric liner (including, for example, silicon nitride, silicon oxide, silicon oxynitride, carbon oxynitride silicon or a combination thereof). In another example, the substrate isolation structure 222 may include a dielectric layer above a doped liner, such as a borosilicate glass (BSG) liner and / or a phosphosilicate glass (PSG) liner. The dimensions and / or characteristics of substrate isolation structure 222 are configured to provide a shallow trench isolation (STI) structure, a deep trench isolation (DTI) structure, a local oxidation of silicon (LOCOS) structure, other suitable isolation structures, or combinations thereof. In the depicted embodiment, substrate isolation structure 222 may be STI.
[0027] The inner spacer 224 is disposed below the gate spacer 240 and along the sidewall of the semiconductor layer 215. The inner spacer 224 is disposed between and separates the semiconductor layer 215 and the source / drain 225. The inner spacer 224 is further disposed between adjacent semiconductor layers 220 and between the bottommost semiconductor layer 220 and the mesa 202'. The inner spacer 224 includes a dielectric material including silicon, oxygen, carbon, nitrogen, other suitable components or combinations thereof, such as silicon nitride, silicon oxynitride, silicon carbide, silicon oxycarbide, silicon carbonitride, etc. In some embodiments, the inner spacer 224 includes a low-k dielectric material. In some embodiments, a dopant (e.g., a p-type dopant, an n-type dopant or a combination thereof) is introduced into the dielectric material, and the inner spacer 224 includes a doped dielectric material.
[0028] The source / drain 225 includes a semiconductor material and may be doped with an n-type dopant and / or a p-type dopant. When forming part of a p-type transistor, the source / drain 225 may include silicon germanium or germanium doped with boron, other p-type dopants, or a combination thereof. When forming part of an n-type transistor, the source / drain 225 may include silicon doped with carbon, phosphorus, arsenic, other n-type dopants, or a combination thereof. The source / drain 225 may include more than one semiconductor layer, wherein the semiconductor layer includes the same or different materials and / or the same or different dopant concentrations. The source / drain 225 may include a material and / or dopant that achieves a desired tensile stress and / or compressive stress in the channel region C. In some embodiments, the source / drain 225 is formed using an epitaxial growth process, and the source / drain 225 may be referred to as an epitaxial source / drain. In some embodiments, doped regions such as heavily doped source / drain (HDD) regions, lightly doped source / drain (LDD) regions, other doped regions, or combinations thereof are disposed in the source / drain 225. In some embodiments, doped regions such as LDD regions may extend into the channel region C. As used herein, source / drain regions, source / drain, source / drain components, etc. may refer to a source of a device, a drain of a device, or sources and / or drains of multiple devices.
[0029] The dummy gate 232 extends longitudinally in a direction different from (e.g., orthogonal to) the length direction of the semiconductor stack 210. For example, the dummy gate 232 extends longitudinally along the y direction, has a length along the y direction, a width along the x direction, and a height along the z direction. Figure 3A In FIG. 2 , a dummy gate 232 is disposed on top of the semiconductor stack 210 . Figure 3BIn the embodiment, the dummy gate 232 is disposed on the top wall and the side wall of the semiconductor stack 210, and the dummy gate 232 wraps the semiconductor stack 210. The dummy gate 232 may include a dummy gate electrode and a dummy gate dielectric. The dummy gate electrode includes a suitable dummy gate material, such as polysilicon (e.g., a polysilicon gate), and the dummy gate dielectric includes a suitable dielectric material, such as silicon oxide (e.g., a dummy oxide). The dummy gate 232 may include additional layers, such as a hard mask layer (e.g., a nitride mask), other suitable layers, or combinations thereof.
[0030] The gate spacer 240 is adjacent to the sidewall of the dummy gate 232 and along the sidewall of the dummy gate. The gate spacer 240 may include a sealing spacer, an offset spacer, a sacrificial spacer, a dummy spacer, a main spacer, other suitable spacers or a combination thereof. The gate spacer 240 may have a single-layer structure or a multi-layer structure. The gate spacer 240 includes a dielectric material, which may include silicon, oxygen, carbon, nitrogen, other suitable components or combinations thereof (e.g., silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, silicon oxycarbide, carbon oxynitride, silicon oxynitride, etc.). For example, the gate spacer 240 may include silicon, oxygen, nitrogen, carbon and hydrogen (i.e., the gate spacer 240 may be a SiONCH layer).
[0031] The dielectric layer 250 is disposed over the substrate 202, the substrate isolation structure 222, the source / drain 225, and the gate structure 230. The dielectric layer 250 may have a multi-layer structure, such as a contact etch stop layer (CESL) 252 and an interlayer dielectric (ILD) layer 254. The ILD layer 254 is formed over the CESL 252. The ILD layer 254 includes a dielectric material, which includes, for example, silicon oxide, carbon-doped silicon oxide, silicon nitride, silicon oxynitride, oxide formed by tetraethyl orthosilicate (TEOS), BSG, PSG, borophosphosilicate glass (BPSG), fluorosilicate glass (FSG), xerogel, aerogel, amorphous fluorinated carbon, polyparaxylene, benzocyclobutene-based (BCB) dielectric material, polyimide, other suitable dielectric materials, or combinations thereof. In some embodiments, the ILD layer 254 includes a dielectric material having a dielectric constant less than that of silicon dioxide (e.g., k<3.9). In some embodiments, the ILD layer 254 includes a dielectric material having a dielectric constant less than about 2.5 (i.e., an extremely low-k dielectric material), such as porous silicon oxide, silicon carbide, a carbon-doped oxide (e.g., a SiCOH-based material (having, for example, Si—CH 3 bonds)), or a combination thereof. The CESL 252 includes a dielectric material different from the dielectric material of the ILD layer 254. For example, in the case where the ILD layer 254 includes silicon and oxygen (e.g., porous silicon oxide), the CESL 252 may include silicon and nitrogen, and the CESL 254 may be a silicon nitride layer, a silicon carbonitride layer, or a silicon carbon nitride oxide layer.
[0032] In some embodiments, the device precursor is received before and / or after the dielectric layer 250 is formed. The formation of the dielectric layer 250 may include depositing a dielectric material over the substrate 202, the substrate isolation structure 222, the source / drain 225, and the gate structure 230, and performing a planarization process, such as chemical mechanical polishing (CMP), on the dielectric material. The planarization process removes any dielectric material from the gate structure 230. The dummy gate 232 may be used as a planarization stop layer, and the planarization process may be performed until the dummy gate 232 is reached. The planarization process may planarize the top surface of the dielectric layer 250 and the top surface of the gate structure 230. In some embodiments, the dielectric layer 250 is a device-level dielectric layer of a multi-layer interconnect (MLI) component that electrically connects devices (e.g., transistors, resistors, capacitors, inductors, etc.), components of the device (e.g., gates and / or source / drains), devices within the MLI component, components of the MLI component, or a combination thereof, so that the device and / or component can operate as specified by the design requirements.
[0033] Go to Figure 1 , Figure 4A and Figure 4B , the method 100 includes, at box 110, removing the dummy gate 232 to form a gate opening 255 exposing the semiconductor stack 210. The gate opening 255 has sidewalls formed by the gate spacer 240 and a bottom formed by the semiconductor stack 210 and / or the substrate isolation structure 222. In some embodiments, the etching process selectively removes the dummy gate 232 relative to the gate spacer 240, the dielectric layer 250, or a combination thereof. For example, the etching process etches the dummy gate 232 without etching (or ignoring) the gate spacer 240, the substrate isolation structure 222, the dielectric layer 250, or a combination thereof. The etchant of the etching process may etch polysilicon (i.e., the dummy gate 232) at a higher rate than the dielectric material (i.e., the gate spacer 240, the substrate isolation structure 222, the dielectric layer 250, etc.). The etching process is dry etching, wet etching, other suitable etching, or a combination thereof. In some embodiments, the patterned mask layer covers the dielectric layer 250 and / or the gate spacer 240, but exposes the dummy gate 232 during the etching process.
[0034] Go to Figure 1 , Figure 5A and Figure 5B, the method 100 at box 115 may include performing a channel release process. For example, the semiconductor layer 215 exposed by the gate opening 255 is selectively removed to form a gap 260 between the semiconductor layers 220 and between the semiconductor layers 220 and the mesas 202', thereby suspending the semiconductor layer 220 in the channel region C. In the described embodiment, three semiconductor layers 220 are vertically stacked in the z direction and provide three channels through which current can flow between the source / drain 225. The suspended semiconductor layer 220 is therefore referred to as the channel layer 220' hereinafter. The channel layer 220' has a width W along the y direction, a thickness T along the z direction, and a spacing S along the z direction. In some embodiments, the width W is about 10nm to about 60nm. In some embodiments, the thickness T is about 5nm to about 10nm. In some embodiments, the spacing S is about 5nm to about 15nm.
[0035] In some embodiments, the channel release process includes an etching process that selectively removes the semiconductor layer 215 relative to the semiconductor layer 220, the mesa 202', the gate spacer 240, the internal spacer 224, the substrate isolation structure 222, the dielectric layer 250, or a combination thereof. For example, the etching process etches the semiconductor layer 215, while not etching (or negligibly) the semiconductor layer 220, the mesa 202', the gate spacer 240, the internal spacer 224, the substrate isolation structure 222, the dielectric layer 250, or a combination thereof. The etchant of the etching process can etch silicon germanium (i.e., the semiconductor layer 215) at a higher rate than silicon (i.e., the semiconductor layer 220) and the dielectric material (i.e., the gate spacer 240, the internal spacer 224, the substrate isolation structure 222, the dielectric layer 250, etc.). The etching process is dry etching, wet etching, other suitable etching processes, or a combination thereof. In some embodiments, before performing the etching process, an oxidation process converts the semiconductor layer 215 into a semiconductor oxide component (e.g., silicon germanium oxide), and then the etching process removes the semiconductor oxide component. In some embodiments, during and / or after removing the semiconductor layer 215, an etching process is performed to change the profile of the semiconductor layer 220 to achieve a target size and / or target shape of the channel layer 220', such as a cylindrical channel layer (e.g., a nanowire), a rectangular channel layer, a sheet-shaped channel layer, etc.
[0036] Go to Figure 1 , Figures 6A-13A and Figure 6B-Figure 13B , the method 100 includes forming a gate stack in the gate opening 255 at block 120. Fig.13A and Fig. 13B , the gate stack includes a gate dielectric 230A (eg, at least one gate dielectric layer) and a gate electrode 230B (eg, at least one conductive gate layer). The gate stack fills the gate opening 255 and, in the depicted embodiment, fills the gap 260 (see FIG. Fig.13A and Fig. 13B ). For example, the gate stack is disposed between the channel layers 220' and between the channel layers 220' and the mesas 202'. Fig.13A In FIG. 1 , the gate stack is disposed between the gate spacers 240 and between the inner spacers 224. Fig. 13B , the gate stack at least partially surrounds (eg, wraps around) the channel layer 220 ′. The gate stack may include more or fewer layers than depicted and described herein. The gate stack and gate spacers 240 are collectively referred to as a gate structure 230 .
[0037] refer to Figure 1 , Fig. 6A and Figure 6B The method 100 includes forming an interface layer 262 at block 125. The interface layer 262 partially fills the gate opening 255 (including the gap 260), and the interface layer 262 is formed over the channel layer 220' and the mesa 202'. The interface layer 262 includes a dielectric material such as SiO2, SiGeO x , HfSiO, SiON, other dielectric materials, or combinations thereof. The interfacial layer 262 partially fills the gate opening 255 (including the gap 260). In some embodiments, the interfacial layer 262 is formed on semiconductor surfaces (e.g., the channel layer 220' and the mesa 202'), but not on dielectric surfaces (e.g., the internal spacer 224, the substrate isolation structure 222, the gate spacer 240, and the dielectric layer 250), as shown. For example, the interfacial layer 262 can be formed by an oxidation process (such as thermal oxidation and / or chemical oxidation), in which oxygen reacts with the semiconductor surface to form a semiconductor oxide (i.e., the interfacial layer 262), but not on the dielectric surface. Fig. 6A In the embodiment, the interface layer 262 covers the top surface of the channel layer 220', the bottom surface of the channel layer 220', and the top surface of the mesa 202'. Figure 6B In some embodiments, the interface layer 262 surrounds the channel layer 220' and wraps around the mesa 202'. In some embodiments, the interface layer 262 is formed by atomic layer deposition (ALD) and / or other suitable methods. In some embodiments, the interface layer 262 has a substantially uniform thickness, such as that depicted. In some embodiments, the interface layer 262 has a thickness of about to about Thickness.
[0038] refer to Figure 1 , Fig. 7A and Figure 7B, the method 100 includes forming a high-k dielectric layer 264 over the interface layer 262 at block 130. The high-k dielectric layer 264 partially fills the gate opening 255 (including the gap 260), and the high-k dielectric layer 264 can be formed over the gate spacer 240, the inner spacer 224, the substrate isolation structure 222, and the dielectric layer 250 (for example, when formed by a conformal deposition process). The high-k dielectric layer 264 includes a high-k dielectric material such as HfO2, HfSiO, HfSiO4, HfSiON, HfLaO, HfTaO, HfTiO, HfZrO, Hf / AlO x , ZrO, ZrO2, ZrSiO2, AlO, AlSiO, Al2O3, TiO, TiO2, LaO, LaSiO, LaO3, La2O3, Ta2O3, Ta2O5, Y2O3, SrTiO3, BaZrO, BaTiO3 (BTO), (Ba, Sr)TiO3 (BST), Si3P4, HfO2-Al2O3, other high-k dielectric materials or combinations thereof. High-k dielectric materials generally refer to dielectric materials having a dielectric constant greater than that of silicon dioxide (k≈3.9). For example, high-k dielectric layer 264 is a hafnium-based oxide (e.g., HfO2) layer or a zirconium-based oxide (e.g., ZrO2) layer. In Fig. 7A In FIG. 2 , the high-k dielectric layer 264 has a u-shaped profile at the top of the gate opening 255 and a rectangular profile at the bottom of the gate opening 225 (ie, in the gap 260 ). Figure 7B In the embodiment, the high-k dielectric layer 264 surrounds the channel layer 220' and wraps the mesa 202'. The high-k dielectric layer 264 is formed by ALD, CVD, physical vapor deposition (PVD), an oxide-based deposition process, other suitable processes or combinations thereof. The thickness of the high-k dielectric layer 264 is greater than the thickness of the interface layer 262. In some embodiments, the thickness of the high-k dielectric layer 264 is about to about In some embodiments, high-k dielectric layer 264 has a substantially uniform thickness, such as depicted.
[0039] refer to Figure 1 , Fig. 8A and Figure 8B , the method 100 includes forming a work function layer 272 on the high-k dielectric layer 264 at block 135. The work function layer 272 partially fills the gate opening 255. In the depicted embodiment, the work function layer 272 partially fills the gap 260. Fig. 8A In FIG. 2 , the work function layer 272 has a u-shaped profile at the top of the gate opening 255 and has a rectangular profile at the bottom of the gate opening 255 (ie, in the gap 260 ). Figure 8BIn the embodiment, the work function layer 272 surrounds the channel layer 220' and wraps the mesa 202'. The thickness of the work function layer 272 is greater than the thickness of the high-k dielectric layer 264. In some embodiments, the thickness of the work function layer 272 is about to about The work function layer 272 is formed by ALD, CVD, PVD, other processes, or combinations thereof. In some embodiments, the work function layer 272 is formed by a conformal deposition process, and the work function layer 272 has a substantially uniform thickness, such as depicted.
[0040] The work function layer 272 is a conductive layer tuned to have a desired work function. The work function layer 272 may be an n-type work function metal (N-WFM) layer, a p-type work function metal (P-WFM), or a combination thereof. The N-WFM layer (also referred to as an n-metal layer) includes an n-type work function material, which generally refers to a conductive material tuned to have an n-type work function, while the P-WFM layer (also referred to as a p-metal layer) includes a p-type work function material, which generally refers to a conductive material tuned to have a p-type work function. The n-type work function material may include a metal having a sufficiently low effective work function, such as aluminum, titanium, tantalum, zirconium, other n-metals, their alloys, or combinations thereof. In some embodiments, the N-WFM layer is a titanium aluminum layer, a titanium aluminum carbide layer, a tantalum carbide layer, a tantalum carbonitride layer, or a tantalum silicon nitride. The p-type work function material may include a metal having a sufficiently high effective work function, such as titanium, tantalum, ruthenium, molybdenum, tungsten, platinum, other p-type metals, their alloys, or combinations thereof. In some embodiments, the P-WFM layer is a titanium nitride layer, a titanium carbide layer, a titanium silicon nitride layer, a tantalum nitride layer, a tungsten carbonitride layer, or a molybdenum layer. In some embodiments, the work function layer has a multilayer structure, such as more than one N-WFM layer, more than one P-WFM layer, or N-WFM and P-WFM. In some embodiments, the work function layer 272 is tuned to have an n-type work function or a p-type work function, depending on the type of transistor to which it belongs. For example, when the device 200 is configured as an n-type transistor, the work function layer 272 can be an N-WFM layer, and when the device 200 is configured as a p-type transistor, the work function layer 270 can be a P-WFM layer.
[0041] In the described embodiment, the work function layer 272 is an N-WFM layer, such as a titanium aluminum carbide (TiAlC) layer formed by ALD. For example, the work function layer 272 includes titanium, aluminum, and carbon, the aluminum concentration / content in the work function layer 272 is about 20 atomic % (at%) to about 40 at%, and the thickness of the work function layer 272 depends on the concentration / content of aluminum in the work function layer 272. For example, in order to maintain a desired threshold voltage, the thickness of the work function layer 272 can be increased or decreased according to the aluminum content in the work function layer 272. The thickness of the work function layer 272 is inversely proportional to the aluminum content in the work function layer 272. Therefore, if the desired threshold voltage corresponds to a work function layer with a given thickness and a given aluminum content, the work function layer 272 is configured to have an aluminum content less than the given aluminum content, and the thickness of the work function layer 272 can be configured to be greater than the given thickness to maintain the desired threshold voltage (i.e., the thickness increases as the aluminum content decreases). If the work function layer 272 is configured to have an aluminum content greater than a given aluminum content, the thickness of the work function layer can be configured to be less than the given thickness to maintain a desired threshold voltage (i.e., the thickness decreases with increasing aluminum content). In some embodiments, the thickness of the work function layer 272 is less than about (For example to about ), and the aluminum content is about 30 at % to about 40 at %. In the depicted embodiment, the work function layer 272 has less than about and greater than approximately (For example, about to about ) and an aluminum content of about 20 at % to about 30 at %. Configuring the work function layer 272 with a lower aluminum content (about 20 at % to about 30 at %) reduces gate resistance, particularly gate resistance associated with inner portions of the gate stack (such as those portions filling the gaps 260 between the channel layers 220 'and / or the gaps 260 between the channel layers 220 'and the mesas 202 ').
[0042] refer to Figure 1 , Figures 9A-11A and Figure 9B-Figure 11B , the method 100 includes forming a cap 274 over the work function layer 272 at block 140. Fig.11A and Fig. 11B In the embodiment, the cap 274 includes a cap layer 276 and a cap layer 278, and the composition of the cap layer 276 is different from the composition of the cap layer 278. For example, the cap layer 276 is a layer including a metal, such as a metal nitride layer, and the cap layer 278 is a layer including a semiconductor, such as a silicon layer. In some embodiments, the method 100 includes forming a metal nitride layer (e.g., the cap layer 276) over the work function layer 272 at block 140 and at block 145 (see Fig.9A , Fig. 9B , Fig. 10A and Fig. 10B ), and forming a silicon-containing layer (eg, cap layer 278) over the metal nitride layer at block 150 (see Fig.11A and Fig. 11B ). Forming the cap layer 276 may include forming a first portion of the cap layer 276A (eg, the cap layer 276A) above the work function layer 272 ( Fig.9A and Fig. 9B ), and after breaking the vacuum, a second portion of the capping layer 278 (e.g., the capping layer 276B) is formed ( Fig. 10A and Fig. 10B ). In the depicted embodiment, since cap layer 276 is a metal nitride layer, cap layer 276A and cap layer 276B are metal nitride sublayers. In some embodiments, cap layer 276 has more than two sublayers, where the vacuum can be broken after forming each sublayer, or the vacuum can be broken after forming some sublayers but not after forming other sublayers. In some embodiments, cap layer 278 has a multilayer structure. In some embodiments, cap 274 has more than two cap layers.
[0043] refer to Fig.9A and Fig. 9B , a cap layer 276A is formed over the work function layer 272. The cap layer 276A partially fills the top of the gate opening 255 and fills the remaining portion of the bottom of the gate opening 225 (i.e., the gap 260). Therefore, the gaps between the channel layers 220' and between the bottommost channel layer 220' and the mesa 202' are filled by the cap layer 276A, the work function layer 272, and the gate dielectric 230A. Fig.9A In FIG. 2 , the capping layer 276A has a U-shaped profile at the top of the gate opening 255 and a rectangular profile at the bottom of the gate opening 255. Fig. 9B In FIG. 2 , the capping layer 276A surrounds the channel layer 220 ′ and wraps the mesa 202 ′.
[0044] The cap layer 276A is a metal nitride layer. The metal nitride layer may include TiN, TiSiN, TaSiN, TaN, TaCN, WN, WCN, other metal nitrides or combinations thereof. In the depicted embodiment, the cap layer 276A includes titanium and nitrogen, and the cap layer 276A may be a TiN sublayer. The cap layer 276A is formed by ALD, CVD, PVD, other suitable processes or combinations thereof. In some embodiments, the cap layer 276A is formed by ALD, and the ALD includes flowing a titanium-containing precursor (e.g., TiCl4) and a nitrogen-containing precursor (e.g., ammonia (NH3)) and / or a hydrogen-containing precursor (e.g., H2) into a process chamber to form a TiN sublayer. In some embodiments, the cap layer 276A is formed by plasma enhanced ALD (PEALD), and the PEALD includes flowing a titanium and nitrogen-containing precursor (e.g., tetrakis(dimethylamino)titanium (TDMAT)) and a hydrogen-containing precursor (e.g., H2 and / or NH3) into a process chamber to form a TiN sublayer. In some embodiments, the cap layer 276A is formed by PEALD, and the PEALD includes flowing a titanium and nitrogen-containing precursor (e.g., TDMAT) into a process chamber to form a TiN sublayer. Parameters of ALD and / or PEALD (e.g., number of cycles, cycle time, temperature, pressure, etc.) and / or other deposition processes may be adjusted to obtain a desired thickness of the cap layer 276A. In some embodiments, the thickness of the cap layer 276A (e.g., the TiN sublayer) is about to about
[0045] The cap layer 276A and the work function layer 272 can be formed "in situ", which generally refers to the process being performed without breaking the vacuum. For example, when forming the work function layer 272 and the cap layer 276A, the device 200 is contained in an environment under vacuum conditions and is maintained in vacuum conditions between forming the work function layer 272 and forming the cap layer 276A. In other words, the vacuum is not broken between forming the work function layer 272 and forming the cap layer 276A, so that the device 200 is not exposed to air (e.g., atmospheric oxygen) between such process steps. In some embodiments, the work function layer 272 and the cap layer 276A are formed in the same process chamber, and the device 200 is maintained under vacuum conditions between forming the work function layer 272 and forming the cap layer 276A. In some embodiments, the work function layer 272 and the cap layer 276A are formed in different process chambers of a semiconductor process tool and / or a semiconductor process system, and the device 200 is maintained under vacuum conditions when it is transferred from the process chamber for forming the work function layer 272 to the process chamber for forming the cap layer 276A. In some embodiments, the work function layer 272 and the cap layer 276A are formed in different semiconductor process tools and / or semiconductor process systems, and the device 200 is maintained under vacuum conditions when moved between semiconductor process tools and / or semiconductor processing systems.
[0046] refer to Fig. 10A and Fig. 10B , a cap layer 276B is formed over the cap layer 276A. The cap layer 276B partially fills the top of the gate opening 255. Fig. 10A In FIG. 2 , the cap layer 276B has a U-shaped profile at the top of the gate opening 255. Fig. 10B In the embodiment, the cap layer 276B wraps around the channel layer 220'. In the embodiment where the cap layer 276A does not fill the remaining portion of the gap 260, the cap layer 276B can partially fill the gap 260 or fill the gap 260. In such an embodiment, the cap layer 276B can also surround the channel layer 220' and / or the cap layer 276B can also wrap around the mesa 202'.
[0047] Cap layer 276B is a metal nitride layer. The metal nitride layer may include TiN, TiSiN, TaSiN, TaN, TaCN, WN, WCN, other metal nitrides or combinations thereof. In the depicted embodiment, cap layer 276B includes the same material as cap layer 276A. For example, cap layer 276B includes titanium and nitrogen, and cap layer 276B may be a TiN sublayer. In some embodiments, cap layer 276B and cap layer 276A include different metal nitride materials. Cap layer 276B is formed by ALD, CVD, PVD, other suitable processes or combinations thereof. In some embodiments, cap layer 276B is formed by ALD, and ALD includes flowing a titanium-containing precursor (e.g., TiCl4) and a nitrogen-containing precursor (e.g., NH3) and / or a hydrogen-containing precursor (e.g., H2) into a process chamber to form a TiN sublayer. In some embodiments, the cap layer 276B is formed by PEALD, and PEALD includes flowing a titanium and nitrogen-containing precursor (e.g., TDMAT) and a hydrogen-containing precursor (e.g., H2 and / or NH3) into a process chamber to form a TiN sublayer. In some embodiments, the cap layer 276B is formed by PEALD, and PEALD includes flowing a titanium and nitrogen-containing precursor (e.g., TDMAT) into a process chamber to form a TiN sublayer. Parameters of ALD and / or PEALD (e.g., number of cycles, cycle time, temperature, pressure, etc.) and / or other deposition processes can be adjusted to obtain the desired thickness of the cap layer 276B. In the depicted embodiment, the thickness of the cap layer 276B is less than the thickness of the cap layer 276A. In some embodiments, the thickness of the cap layer 276B (e.g., the TiN sublayer) is about to about In some embodiments, the total thickness of the capping layer 276 (eg, the sum of the thickness of the capping layer 276A and the thickness of the capping layer 276B) is about 1000 Å. to about
[0048] Cap layer 276B and cap layer 276A are formed "ex situ", which generally refers to breaking vacuum between processes. For example, when forming cap layer 276A and forming cap layer 276B, device 200 is contained in an environment under vacuum conditions, but device 200 is not kept under vacuum conditions (i.e., device 200 can be exposed to oxygen) between forming cap layer 276A and forming cap layer 276B. In other words, vacuum is broken between forming cap layer 276A and forming cap layer 276B, so that device 200 is exposed to air (e.g., atmospheric oxygen) between these process steps. In some embodiments, cap layer 276A and cap layer 276B are formed in the same process chamber, and vacuum is broken between forming cap layer 276A and forming cap layer 276B. In some embodiments, the capping layer 276A and the capping layer 276B are formed in different process chambers of a semiconductor process tool and / or a semiconductor process system, and the vacuum is broken when the device 200 is transferred from the process chamber for forming the capping layer 276A to the process chamber for forming the capping layer 276B. In some embodiments, the capping layer 276A and the capping layer 276B are formed in different semiconductor process tools and / or different semiconductor processing systems, and the vacuum is broken when the device 200 is transferred between semiconductor process tools and / or semiconductor processing systems.
[0049] Because the vacuum is broken when forming the cap layer 276, the cap layer 276 is referred to as an ex situ cap layer, and the cap 274 is referred to as an ex situ cap. In some embodiments, before forming the cap layer 276B, the vacuum is broken to expose the cap layer 276A to an oxygen environment. For example, when the vacuum is broken (i.e., the device 200 is no longer in a vacuum-regulated environment), the cap layer 276A is exposed to air (e.g., atmospheric oxygen), and the cap layer 276A adsorbs oxygen from the oxygen environment, and the oxygen can be combined with the metal to provide a cap layer 276A having a metal-oxygen bond. Due to the adsorption of oxygen by the cap layer 276A, the exposed surface of the cap layer 276A can be converted into a thin metal oxide layer and / or a thin metal oxynitride layer, which is depicted as an oxidized surface 276O (also referred to as an oxide layer 276O). The oxide layer 276O may include a metal-oxygen bond, a metal-nitrogen bond, a metal-oxygen-nitrogen bond, or a combination thereof. In some embodiments, the oxide layer 276O of the cap layer 276A has a thickness of about 0.1 nm to about 0.2 nm. In embodiments where the cap layer 276A includes metal-oxygen bonds before the vacuum is broken, such as embodiments where the cap layer 276A includes oxygen and / or where oxygen has diffused into the cap layer 276A during processing of the device 200, the metal-oxygen bonds of the cap layer 276A can increase when the cap layer 276A adsorbs oxygen from an oxygen environment. Forming and / or increasing metal-oxygen bonds in the cap layer 276A reduces and / or repairs oxygen vacancies therein (which can mitigate oxygen diffusion from the cap 274 and / or subsequently formed layers into the work function layer 272 and the gate dielectric 230A during fabrication of the device 200), thereby reducing unintentional oxidation and minimizing threshold voltage changes and / or other device performance changes (e.g., reductions in speed and / or mobility) caused by such oxidation. In addition, reducing and / or repairing oxygen vacancies can reduce gate resistance. In the depicted embodiment, where the cap layer 276A is a TiN sublayer, the TiN sublayer adsorbs oxygen from the oxygen environment, which forms and / or increases Ti-O bonds of the TiN sublayer. In such an embodiment, the oxide layer 276O and / or the cap layer 276A may include Ti-N bonds, Ti-O bonds, Ti-ON bonds, or a combination thereof.
[0050] refer to Fig.11A and Fig. 11B , a capping layer 278 is formed over the capping layer 276, such as over the capping layer 276B. The capping layer 278 partially fills the top of the gate opening 255. Fig.11A In FIG. 2 , the capping layer 278 has a U-shaped profile at the top of the gate opening 255. Fig. 11BIn the embodiment, the capping layer 278 wraps around the channel layer 220'. In the embodiment where the capping layer 276 does not fill the remaining portion of the gap 260, the capping layer 278 may partially fill the gap 260 or fill the remaining portion of the gap 260. In such an embodiment, the capping layer 278 may wrap around the channel layer 220' and / or the capping layer 278 wraps around the mesa 202'.
[0051] The cap layer 278 includes a material with a strong oxygen affinity, which can prevent oxygen from diffusing into the work function layer 272 and mitigate the threshold voltage shift that may be caused by the oxidation of the work function metal. For example, the cap layer 278 is a silicon-containing layer. The silicon-containing layer may include silicon, polysilicon, amorphous silicon, or a combination thereof. In the depicted embodiment, the cap layer 278 is a silicon layer. The cap layer 278 is formed by ALD, CVD, PVD, other suitable processes, or a combination thereof. In some embodiments, the cap layer 278 is formed by soaking in silane (SiH4). In some embodiments, the cap layer 278 is formed by CVD or ALD, and the CVD of the ALD includes flowing a silicon-containing precursor (e.g., SiH4 and / or disilane (Si2H6)) and a hydrogen-containing precursor (e.g., H2) into the process chamber to form a silicon layer. The parameters of the deposition process (e.g., precursors, time, temperature, pressure, etc.) can be adjusted to obtain the desired thickness of the cap layer 278. In the depicted embodiment, the thickness of the capping layer 278 can be less than the thickness of the capping layer 276. In some embodiments, the thickness of the capping layer 278 is about to about In some embodiments, the thickness of the cap layer 278 is greater than the thickness of the cap layer 276. In some embodiments, the sum of the thickness of the cap layer 276 and the thickness of the cap layer 278 (ie, the thickness of the cap 274) is about to about
[0052] Cap layer 278 and cap layer 276B can be formed in situ. For example, when forming cap layer 278 and cap layer 276B, device 200 is contained in a vacuum-regulated environment, and device 200 is kept under vacuum conditions between forming cap layer 278 and forming cap layer 276B. In other words, vacuum is not destroyed between forming cap layer 278 and forming cap layer 276B, so that device 200 is not exposed to air between process steps. In some embodiments, cap layer 278 and cap layer 276B are formed in the same process chamber, and device 200 is kept under vacuum conditions between forming cap layer 278 and forming cap layer 276B. In some embodiments, cap layer 278 and cap layer 276B are formed in different process chambers of semiconductor process tool and / or semiconductor process system, and device 200 is kept under vacuum conditions when transferring between them. In some embodiments, cap layer 278 and cap layer 276B are formed in different semiconductor process tools and / or different semiconductor processing systems. In such embodiments, the device 200 may be maintained under vacuum conditions as it moves between them.
[0053] refer to Figure 1 , Fig. 12A , Fig. 12B , Fig.13A and Fig. 13B , the method 100 includes forming a fluorine-free tungsten (FFW) layer 280 over the cap 274 at block 160. The FFW layer 280 fills the remaining portion of the gate opening 255, and the FFW layer 280 may be referred to as a bulk (filling) layer of the gate stack. In the depicted embodiment, the FFW layer 280 is disposed directly on and physically contacts the cap layer 278. Because the cap 274, the work function layer 272, and the gate dielectric 230A fill the gap 260, the FFW layer 280 is not substantially larger than the gate stack in the XZ cross-sectional view ( Fig. 12A and Fig.13A ) has a u-shaped profile at the top of the gate opening 255 and wraps the channel layer 220' ( Fig. 12B and Fig. 13B ). In embodiments where the cap 274 does not fill the remainder of the gap 260, the FFW layer 280 may fill the remainder of the gap 260. In such embodiments, the FFW layer 280 surrounds the channel layer 220' and / or the FFW layer 280 wraps around the mesa 202'. In some embodiments, the thickness of the FFW layer 280 is about to about
[0054] refer to Fig. 12A and Fig. 12B, forming the FFW layer 280 includes depositing the FFW material on the cap layer 278 (e.g., silicon layer) by ALD, CVD, PVD, other suitable processes, or combinations thereof. Since the FFW material may not be easy to grow / deposit on silicon oxide, the FFW layer 280 and the cap layer 278 are formed in situ. For example, referring to Fig.14A If the capping layer 278 and the FFW layer 280 are formed ex-situ (i.e., the vacuum is broken between the formation of the capping layer 278 and the FFW layer 280), the capping layer 278 may be exposed to air (e.g., atmospheric oxygen) and / or other oxygen environments, and the capping layer 278 may absorb oxygen from the air and / or other oxygen environments. Since the capping layer 278 adsorbs oxygen, the oxygen may combine with silicon to form silicon-oxygen bonds, and the exposed top surface of the capping layer 278 (on which the FFW layer 280 is formed) may be oxidized and converted into a thin silicon oxide layer 278O, from which the FFW material may not be easily grown / deposited. For example, because the FFW material deposition / growth rate is inversely proportional to the electronegativity of the surface on which the FFW material is deposited / grown (e.g., as the electronegativity of the deposition / growth surface decreases, the FFW material deposition / growth increases), and the electronegativity of silicon oxide is greater than the electronegativity of silicon, the deposition / growth of the FFW material on silicon will be faster than on silicon oxide, and the incubation time / cycle for tungsten grown / deposited on silicon is less than the incubation time / cycle for tungsten grown / precipitated on silicon oxide. In some cases, the FFW material may not be deposited / grown on silicon oxide. For example, the tungsten-containing compound 282 (e.g., WCl5) of the tungsten-containing precursor used to deposit the FFW material may not react with the silicon oxide layer 278O, or react too slowly.
[0055] Therefore, reference Fig. 14B, in order to enable the FFW layer 280 to be deposited / grown on the cap layer 278, the FFW layer 280 and the cap layer 278 are formed in situ (i.e., the vacuum is not broken between the formation of the cap layer 278 and the FFW layer 280). The in-situ formed FFW layer 280 reduces and / or prevents oxidation of the cap layer 278, which inhibits the formation of a silicon oxide surface / layer 278O on the cap layer 278 and improves the deposition and / or growth of the FFW layer 280 on the cap layer 278. For example, a tungsten-containing compound 282 of a tungsten-containing precursor used to deposit the FFW material can easily react with the silicon surface of the cap layer 278. Therefore, when the cap layer 278 and the FFW layer 280 are formed, the device 200 is contained in a vacuum-regulated environment and is maintained under vacuum conditions between the formation of the cap layer 278 and the formation of the FFW layer 280. In other words, the device 200 is not exposed to an oxygen environment between such process steps. In some embodiments, the capping layer 278 and the FFW layer 280 are formed in the same process chamber, and the device 200 is maintained under vacuum conditions between forming the capping layer 278 and forming the FFW layer 280. In some embodiments, the capping layer 278 and the FFW layer 280 are formed in different process chambers of a semiconductor process tool and / or a semiconductor process system, and the device 200 is maintained under vacuum conditions when transferred from a process chamber for forming the capping layer 278 to a process chamber for forming the FFW layer 280. In some embodiments, the capping layer 278 and the FFW layer 280 are formed in different semiconductor process tools and / or semiconductor process systems, and the device 200 is maintained under vacuum conditions when moved between semiconductor process tools and / or semiconductor processing systems.
[0056] Depositing the FFW material includes flowing a fluorine-free, tungsten-containing precursor into the process chamber, which reacts with the cap layer 278 to form the FFW material. For example, the tungsten-containing precursor is tungsten pentachloride (WCl5), and the WCl5 reacts with the cap layer 278 to form the FFW material. Fig.15A When the capping layer 278 is a silicon layer with a silicon surface on which the FFW material is grown / deposited, it has been observed that silicon loss occurs when WCl5 reacts with silicon (Si) of the capping layer 278, thereby undesirably reducing the thickness of the capping layer 278. For example, when WCl5 accepts electrons from the silicon layer, the W-Cl bond of WCl5 may break, resulting in W bonding to the silicon layer, and the Si-Si bond may break, resulting in silicon and chlorine-containing byproducts, such as SiCl. x H y or SiCl x (e.g. SiCl4), as a bond between Si and Cl. Fig. 15BTo reduce this silicon loss of the cap layer 278, the FFW material is deposited by co-flowing WCl5 (a tungsten-containing precursor) and a hydrogen-containing precursor (e.g., H2) into the process chamber, which reduces the surface reaction between WCl5 and the cap layer 278. For example, WCl5 can react with H2 to form WCl3 and HCl (e.g., WCl5+H2→WCl3+2HCl), and WCl3 can react with the silicon of the cap layer 278. When WCl3 accepts electrons from HCl, in addition to electrons from the silicon layer, the W-Cl bond of WCl3 may be broken, resulting in W bonding to the silicon layer, and the Si-Si bond may be broken, resulting in silicon and chlorine-containing byproducts, such as SiCl x H y or SiCl x (e.g., SiCl4), as a bond of Si to Cl. Since WCl5 may react with H2 (thereby decomposing into WCl3 and HCl), and WCl3 may react with HCl, the reaction between the tungsten-containing compound (e.g., WCl5 and / or WCl3) and the silicon layer results in silicon loss, for example, silicon of the capping layer 278 combines with chlorine to form silicon and chlorine byproducts. Therefore, the silicon loss of the capping layer 278 when WCl5 and H2 are co-flowed to form the FFW material is less than the Si loss of the capping layer 278 when WCl5 is flowed alone to form the FFW material. In some embodiments, the FFW layer 280 is deposited by ALD, and the ALD includes co-flowing a fluorine-free tungsten-containing precursor (e.g., WCl5) and a hydrogen-containing precursor (e.g., H2) into a process chamber to form the FFW layer 280. In some embodiments, the FFW layer 280 is deposited by ALD, and the ALD includes co-flowing a tungsten-containing precursor (eg, WF 6 ) and a hydrogen-containing precursor (eg, H 2 ) into a process chamber to form the FFW layer 280 .
[0057] refer to Fig.13A and Fig. 13B , a planarization process may be performed to remove excess gate material, such as gate material disposed over the dielectric layer 250. For example, a CMP process is performed that removes portions of the FFW layer 280, the cap 274 (e.g., the cap layer 276 and the cap layer 278), the work function layer 272, and the high-k dielectric layer 264 disposed over the dielectric layer 250. The CMP process may be performed until the top surface of the dielectric layer 250 is reached and / or exposed. In some embodiments, the CMP process is continued and the thickness of the dielectric layer 250 is reduced, and the height of the gate structure 230 is correspondingly reduced. In the depicted embodiment, the top of the gate structure 230 is substantially planar with the top of the dielectric layer 250 after the CMP process, and the remaining portion of the gate material filling the gate opening 255 forms a gate stack in the gate structure 230.
[0058] Thus, method 100 provides device 200 with a gate stack having a gate dielectric 230A (e.g., interface layer 262 and high-k dielectric layer 264) and a gate electrode 230B (e.g., FFW layer 280 (i.e., bulk / filling layer), cap 274 (e.g., cap layer 276 and cap layer 278), and work function layer 272). Since gate dielectric layer 230A includes high-k dielectric layer 264, the gate stack may be referred to as a high-k / metal gate. Configuring the gate stack with an in-situ FFW layer (e.g., FFW layer 280) and a work function layer having a low aluminum content (e.g., work function layer 172) reduces the overall resistance (R) of the gate of the transistor (e.g., device 200). g ). For example, the in-situ FWW layer can reduce the gate resistance attributed to the top of the gate stack (i.e., the portion above the top channel layer 220'), and the low aluminum content work function layer can reduce the resistance attributed to the inside of the gate stack (i.e., the portion between the channel layers 220' (i.e., the portion filling the gap 260)). When compared to a device having a gate stack configured with an ex-situ FFW layer and a low aluminum content work function layer, the gate stack of device 200 can reduce the resistance attributed to the top of the gate stack by about 15% and provide a comparable resistance attributed to the inside of the gate stack. In addition, when compared to a device having a gate stack configured with no FFW layer and a high aluminum content (e.g., greater than 30at%) work function layer, the gate stack of device 200 can reduce the resistance attributed to the top of the gate stack by about 20%, and reduce the resistance attributed to the inside of the gate stack by about 50%. Such a resistance reduction can significantly reduce the overall gate resistance, which can improve device performance (e.g., by increasing speed). Such a resistance reduction can be achieved while maintaining a desired threshold voltage. Different embodiments may have different advantages, and no particular advantage is required for any embodiment.
[0059] In some embodiments, reference Fig.16A and Fig. 16B , capping layer 276 is formed without breaking vacuum, and capping layer 276 does not include an oxidized surface / layer 276. In such an embodiment, capping layer 276 may have sub-layers, such as capping layer 276A and capping layer 276B, but vacuum is not broken between forming capping layer 276A and capping layer 276B (i.e., capping layer 276A is not exposed to air and / or other oxygen environments before forming capping layer 276B). In some embodiments, capping layer 276 may not have sub-layers, and capping layer 276 may be formed by depositing a metal nitride layer having a desired thickness over work function layer 272 under vacuum conditions.
[0060] In some embodiments, reference Fig.17A and Fig. 17B, the size of the gate opening 255, the thickness of the work function layer 272, the thickness of the high-k dielectric layer 264, the thickness of the interface layer 262, the size of the channel layer 220', or a combination thereof are configured such that the work function layer 272 fills the remaining portion of the gap 260. In such an embodiment, in the YZ cross-sectional view, the capping layer 276 (e.g., the capping layer 276A and the capping layer 276B) wraps around but does not surround the channel layer 220' ( Fig. 17B ). Therefore, the capping layer 276 is not between the channel layers 220' and / or between the channel layer 220' and the mesa 202'. In other words, the capping layer 276 is not disposed in the inner region of the gate stack.
[0061] In some embodiments, the processing may further include etching back the gate electrode 230B and / or the gate dielectric 230A, and forming a hard mask, such as a self-aligned cap (SAC), over the etched back gate electrode 230B and / or the gate dielectric 230A. The hard mask includes a material different from the dielectric layer 250 and / or the dielectric layer formed thereon to achieve etching selectivity during a subsequent etching process. In some embodiments, the hard mask includes silicon and nitrogen and / or carbon, such as silicon nitride, silicon oxynitride, silicon carbide, silicon oxycarbide, silicon carbonitride, silicon carbon oxynitride, other silicon nitrides, other silicon carbides, or combinations thereof. In some embodiments, the hard mask includes a metal and oxygen and / or nitrogen, such as aluminum oxide, aluminum nitride, aluminum oxynitride, zirconium oxide, zirconium nitride, hafnium oxide, zirconium aluminum oxide, other metal oxides, other metal nitrides, or combinations thereof.
[0062] In some embodiments, reference Figure 1 , Figures 18A-20A and Figure 18B - Figure 20B , method 100 includes at block 160 ( Fig.19A , Fig.19B , Fig. 20A and Fig. 20B ) before forming the FFW layer 280 at frame 155 ( Fig.18A and Fig.18B ) forms a glue layer 290 above the cap 274. Fig.18A and Fig.18B , a glue layer 290 is formed on the cap layer 278. The glue layer 290 partially fills the top of the gate opening 255. Fig.18A In FIG. 2 , the glue layer 290 has a U-shaped profile at the top of the gate opening 255 . Fig.18B In the embodiment, the glue layer 290 wraps around the channel layer 220'. In the embodiment where the cap 274 does not fill the remaining portion of the gap 260, the glue layer 290 may partially fill the gap 260 or fill the remaining portion of the gap 260. In such an embodiment, the glue layer 290 may surround the channel layer 220' and / or the glue layer 290 wraps around the mesa 202'.
[0063] The glue layer 290 may include a material that promotes adhesion between adjacent layers, such as adhesion between the cap 274 and the FFW layer 280, and / or a material that prevents or eliminates diffusion and / or reaction of components between adjacent layers. For example, the glue layer 290 includes a metal and nitrogen, such as TiN, TaN, W2N, TiSiN, TaSiN, other suitable metal nitride materials, or combinations thereof. In the depicted embodiment, the glue layer 290 is a TiN layer. The glue layer 290 is formed by ALD, CVD, PVD, other processes, or combinations thereof. In some embodiments, the thickness of the glue layer 290 is about 1000 Å. to about In some embodiments, glue layer 290 may have a substantially uniform thickness, such as depicted.
[0064] The glue layer 290 and the cap layer 278 can be formed in situ or non-situ. The in-situ formation of the glue layer 290 can reduce the gate resistance. In some embodiments, when the cap layer 278 and the glue layer 290 are formed, the device 200 is contained in an environment under vacuum conditions, and the device 200 is kept in a vacuum condition between the formation of the cap layer 278 and the formation of the glue layer 290. In some embodiments, when the cap layer 278 is formed and when the glue layer 290 is formed, the device 200 is contained in an environment under vacuum conditions, but the device 200 is not kept in a vacuum condition between the formation of the cap layer 278 and the formation of the glue layer 290. In some embodiments, the cap layer 278 and the glue layer 290 are formed in the same process chamber. In some embodiments, the cap layer 278 and the glue layer 290 are formed in different process chambers of a semiconductor process tool and / or a semiconductor process system. In some embodiments, the cap layer 278 and the glue layer 290 are formed in different semiconductor process tools and / or different semiconductor processing systems.
[0065] refer to Fig.19A , Fig.19B , Fig. 20A and Fig. 20B , and then processing can be performed to deposit the FFW layer 280 ( Fig.19A and Fig.19B ), for example as described above, and flattened ( Fig. 20A , Fig. 20B ), such as described above. The planarization process may remove portions of the FFW layer 280, the glue layer 290, the cap 274 (e.g., the cap layer 276 and the cap layer 278), the work function layer 272, and the high-k dielectric layer 264 disposed above the dielectric layer 250. In such an embodiment, the gate stack includes the gate dielectric 230A (e.g., the interface layer 262 and the high-k dielectric layer 264) and the gate electrode 230B (e.g., the FFW layer 280, the glue layer 290, the cap 274 (e.g., the cap layer 276 and the cap layer 278), and the work function layer 272).
[0066] The gate stacks disclosed herein can be applied in various IC applications. For example, a gate stack having an in-situ FFW layer (e.g., FFW layer 280), a silicon-containing cap (e.g., cap layer 278 of cap 274), and a work function layer having a low aluminum content (e.g., work function layer 172) as described herein can be implemented in an inverter. Fig.21 An example circuit schematic diagram of part or all of an inverter 300 according to various aspects of the present disclosure is shown. The inverter 300 includes an inverter 305A electrically connected to an inverter 305B. The inverter 305A and the inverter 305B can each be a complementary metal oxide semiconductor (CMOS) inverter, each of which includes a pair of transistors, such as a corresponding n-type transistor (e.g., transistor N1 or transistor N2) and a corresponding p-type transistor (e.g., transistor P1 or transistor P2). The drains of transistor P1 and transistor N1 are coupled together, the gates of transistors P1 and N1 are coupled together and further coupled to an input node IN, the source of transistor P1 is coupled to a power supply voltage VDD, and the source of transistor N1 is connected to a voltage VSS, which can be an electrical ground. The drains of transistors P2 and N2 are coupled together and further coupled to the output node OUT, the gates of transistors P2 and N2 are coupled together and further coupled to the drains of transistors P1 and P2, the source of transistor P2 is coupled to the power supply voltage VDD, and the source of transistor N2 is coupled to the voltage VSS. Transistor N1 and transistor N2 may be NMOS transistors, and transistor P1 and transistor P2 may be PMOS transistors. For the sake of clarity, the diagram is simplified. Fig.21 To better understand the inventive concepts of the present disclosure. Additional components may be added to the inverter 300, and some of the components described below may be replaced, modified, or eliminated in other embodiments of the inverter 300.
[0067] The inverter 300 can be implemented in a ring oscillator (RO) device and / or a RO circuit, and the RO device can be used to evaluate the performance of transistors, such as transistors configured with a gate stack having an in-situ FFW layer and a low aluminum content work function layer as described herein. In some cases, when its inverter has a transistor configured with a gate stack (the gate stack has an in-situ FFW layer and a low aluminum content work function layer as described herein), the RO speed can be increased by about 2% to about 3%. In some embodiments, the inverter 300 and / or the RO device including the inverter 300 The transistor N1, the transistor N2, the transistor P1, the transistor P2, or a combination thereof has a gate stack configured the same as the gate stack of the device 200 described above, which increases its speed.
[0068] Device 200 may be included in a microprocessor, a memory, an IC, or a combination thereof. Device 200 may be part of an IC chip, a system on a chip (SoC), or a portion thereof, and may include various passive and active microelectronic devices, such as transistors, resistors, capacitors, inductors, diodes, p-type FETs (PFETs), n-type FETs (NFETs), metal oxide semiconductor FETs (MOSFETs), CMOS transistors, bipolar junction transistors (BJTs), laterally diffused MOS (LDMOS) transistors, high voltage transistors, high frequency transistors, other suitable components and / or devices, or a combination thereof.
[0069] The present disclosure provides many different embodiments. A gate stack (e.g., a high-k / metal gate) of a multi-gate device having an in-situ fluorine-free tungsten layer (e.g., FFW layer 280), a silicon-containing cap (e.g., cap layer 278), and a low aluminum content work function layer (e.g., work function layer 272) and a method for manufacturing the same are described herein, and many advantages are provided. The gate stack disclosed herein can be implemented in a variety of device types. For example, the gate stack described herein is suitable for planar field effect transistors (FETs), multi-gate transistors such as FinFETs, GAA transistors, Ω-gate devices, π-gate devices, fork-piece devices, or combinations thereof, as well as strained semiconductor devices, silicon-on-insulator (SOI) devices, partially depleted SOI devices, fully depleted SOI devices, other devices, or combinations thereof.
[0070] An exemplary method for forming a gate stack of a multi-gate device includes forming a gate dielectric over a channel layer and forming a gate electrode over the gate dielectric. The gate electrode is formed by forming a work function layer over the gate dielectric and forming a cap over the work function layer. Forming the cap includes forming a metal nitride layer over the work function layer and forming a silicon-containing layer over the metal nitride layer. The gate electrode is further formed by forming a fluorine-free tungsten layer over the silicon-containing layer of the cap without breaking vacuum. Forming the fluorine-free tungsten layer over the silicon-containing layer includes co-flowing a tungsten-containing precursor and a hydrogen-containing precursor. In some embodiments, the tungsten-containing precursor is WCl5 and the hydrogen-containing precursor is H2.
[0071] In some embodiments, the thickness of the fluorine-free tungsten layer is greater than the thickness of the silicon-containing layer. In some embodiments, the work function layer has an aluminum content of about 20% to about 30% and about to about In some embodiments, the metal nitride layer includes titanium and nitrogen, and the work function layer includes titanium, aluminum, and carbon.
[0072] In some embodiments, forming the metal nitride layer includes: forming a first metal nitride sublayer above the work function layer; and forming a second metal nitride sublayer above the first metal nitride sublayer. In some embodiments, the second metal nitride sublayer is formed on the first metal nitride sublayer after breaking the vacuum.
[0073] In some embodiments, the channel layer is a first channel layer, a gate dielectric is formed above the first channel layer and the second channel layer, and the method further includes forming a gate dielectric and a gate electrode in a gate opening exposing the first channel layer and the second channel layer. The gate dielectric, the work function layer, and the cap fill the gap between the first channel layer and the second channel layer. The gate dielectric, the work function layer, the cap, and the fluorine-free tungsten layer fill the portion of the gate opening above the first channel layer. In some embodiments, the gap (e.g., spacing S) is about 10 nm.
[0074] In some embodiments, the channel layer is a first channel layer, a gate dielectric is formed on the first channel layer and the second channel layer, and the method further includes forming a gate dielectric and a gate electrode in a gate opening exposing the first channel layer and the second channel layer. The gate dielectric and the work function layer fill the gap between the first channel layer and the second channel layer. The gate dielectric, the work function layer, the cap, and the fluorine-free tungsten layer fill a portion of the gate opening on the first channel layer. In some embodiments, the gap (e.g., spacing S) is about 10 nm.
[0075] In some embodiments, the channel layer is a first channel layer; a gate dielectric is formed above the first channel layer and the second channel layer; and the method also includes forming a gate dielectric and a gate electrode in a gate opening exposing the first channel layer and the second channel layer, wherein: the gate dielectric and the work function layer fill the gap between the first channel layer and the second channel layer, and the gate dielectric, the work function layer, the cap, and the fluorine-free tungsten layer fill a portion of the gate opening above the first channel layer.
[0076] In some embodiments, the thickness of the fluorine-free tungsten layer is greater than the thickness of the silicon-containing layer.
[0077] In some embodiments, the work function layer has an aluminum content of about 20% to about 30% and about to about Thickness.
[0078] Another exemplary method includes forming an interfacial layer over a first channel layer and a second channel layer. The first channel layer is disposed over the second channel layer. The method also includes forming a high-k dielectric layer over the interfacial layer, forming a titanium aluminum carbide layer over the high-k dielectric layer; forming a titanium nitride layer over the titanium aluminum carbide layer; forming a silicon layer over the titanium nitride layer, and co-flowing WCl5 and H2 into a process chamber to form an in-situ fluorine-free tungsten layer over the silicon layer. In some embodiments, the interfacial layer, the high-k dielectric layer, and the titanium aluminum carbide layer fill a space between the first channel layer and the second channel layer.
[0079] In some embodiments, the in-situ fluorine-free tungsten layer is formed directly on the silicon layer. In some embodiments, the titanium nitride layer is a first titanium nitride layer, and the method further comprises forming a second titanium nitride layer over the silicon layer, wherein the in-situ fluorine-free tungsten layer is formed directly on the second titanium nitride layer.
[0080] In some embodiments, forming a titanium aluminum carbide layer over the high-k dielectric layer includes: performing an atomic layer deposition process; and adjusting parameters of the atomic layer deposition process to provide a titanium aluminum carbide layer having an aluminum content of about 20% to about 30% and a thickness of about to about In some embodiments, forming a titanium nitride layer on the titanium aluminum carbide layer includes: forming a first titanium nitride sublayer on the titanium aluminum carbide layer; and forming a second titanium nitride sublayer on the first titanium nitride sublayer. In some embodiments, forming a titanium nitride layer on the titanium aluminum carbide layer also includes exposing the first titanium nitride sublayer to an oxygen environment before forming the second titanium nitride sublayer.
[0081] An exemplary transistor includes: a first channel layer and a second channel layer, a gate dielectric surrounding the first channel layer and the second channel layer, and a gate electrode disposed above the gate dielectric. The gate electrode surrounds the first channel layer and the second channel layer. The gate dielectric includes an interface layer and a high-k dielectric layer. The gate electrode includes a titanium aluminum carbide layer disposed above the high-k dielectric layer. The titanium aluminum carbide layer has an aluminum content of about 20% to about 30% and an aluminum content of about to about The gate electrode also includes a cap disposed above the titanium aluminum carbide layer. The cap includes a metal nitride layer disposed above the titanium aluminum carbide layer and a silicon layer disposed above the metal nitride layer. The gate electrode also includes a fluorine-free tungsten layer directly on the silicon layer. In some embodiments, the interface layer, the high-k dielectric layer, the titanium aluminum carbide layer, and the metal nitride layer of the cap fill the gap between the first channel layer and the second channel layer (e.g., about 10 nm). In some embodiments, the interface layer, the high-k dielectric layer, and the titanium aluminum carbide layer fill the gap between the first channel layer and the second channel layer (e.g., about 10 nm).
[0082] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art will appreciate that they can easily use the present disclosure as a basis for designing or modifying other processes and structures for achieving the same purpose of the embodiments introduced herein and / or achieving the same advantages thereof. Those skilled in the art will also appreciate that such equivalent structures do not deviate from the spirit and scope of the present disclosure, and that they can make various changes, substitutions, and changes in the present disclosure without departing from the spirit and scope of the present disclosure.
Claims
1. A method of forming a gate stack of a multi-gate device, the method comprising: forming a gate dielectric over the channel layer; as well as A gate electrode is formed over the gate dielectric by the following steps: a square work function layer on the gate dielectric, forming a cap over the work function layer, wherein forming the cap comprises forming a metal nitride layer over the work function layer and forming a silicon-containing layer over the metal nitride layer, and A fluorine-free tungsten layer is formed over the silicon-containing layer of the cap without breaking vacuum, wherein forming the fluorine-free tungsten layer over the silicon-containing layer includes co-flowing a tungsten-containing precursor and a hydrogen-containing precursor.
2. The method according to claim 1, wherein: The tungsten-containing precursor is WCl5; and The hydrogen-containing precursor is H2.
3. The method according to claim 1, wherein: The metal nitride layer includes titanium and nitrogen, and the work function layer includes titanium, aluminum, and carbon.
4. The method according to claim 1, wherein: Forming the metal nitride layer comprises: forming a first metal nitride sublayer over the work function layer; and A second metal nitride sub-layer is formed over the first metal nitride sub-layer.
5. The method according to claim 1, wherein: The channel layer is a first channel layer; The gate dielectric is formed over the first channel layer and the second channel layer; and The method further includes forming the gate dielectric and the gate electrode in a gate opening exposing the first channel layer and the second channel layer, wherein: The gate dielectric, the work function layer and the cap fill a gap between the first channel layer and the second channel layer, and The gate dielectric, the work function layer, the cap, and the fluorine-free tungsten layer fill a portion of the gate opening above the first channel layer.
6. The method according to claim 1, wherein: The channel layer is a first channel layer; The gate dielectric is formed over the first channel layer and the second channel layer; and The method further includes forming the gate dielectric and the gate electrode in a gate opening exposing the first channel layer and the second channel layer, wherein: The gate dielectric and the work function layer fill a gap between the first channel layer and the second channel layer, and The gate dielectric, the work function layer, the cap, and the fluorine-free tungsten layer fill a portion of the gate opening above the first channel layer.
7. A method of forming a gate stack of a multi-gate device, the method comprising: forming an interface layer over a first channel layer and a second channel layer, wherein the first channel layer is disposed over the second channel layer; forming a high-k dielectric layer over the interface layer; forming a titanium aluminum carbide layer over the high-k dielectric layer; forming a titanium nitride layer on the titanium aluminum carbide layer; forming a silicon layer over the titanium nitride layer; and WCl5 and H2 are co-flowed into the process chamber to form an in-situ fluorine-free tungsten layer over the silicon layer.
8. The method according to claim 7, wherein: The titanium nitride layer is a first titanium nitride layer, and the method further includes forming a second titanium nitride layer over the silicon layer, wherein the in-situ fluorine-free tungsten layer is formed directly on the second titanium nitride layer.
9. The method according to claim 7, wherein: Forming the titanium aluminum carbide layer above the high-k dielectric layer comprises: performing an atomic layer deposition process; and The parameters of the atomic layer deposition process are adjusted to provide an aluminum content of about 20% to about 30% and a thickness of about to about of titanium aluminum carbide layer.
10. A transistor comprising: a first channel layer and a second channel layer; a gate dielectric surrounding the first channel layer and the second channel layer, wherein the gate dielectric comprises an interface layer and a high-k dielectric layer; and a gate electrode disposed above the gate dielectric, wherein the gate electrode surrounds the first channel layer and the second channel layer, wherein the gate electrode comprises: a titanium aluminum carbide layer disposed on the high-k dielectric layer and a cap disposed on the titanium aluminum carbide layer, wherein the cap comprises a metal nitride layer disposed on the titanium aluminum carbide layer and a silicon layer disposed on the metal nitride layer, and A fluorine-free tungsten layer is directly located on the silicon layer.