Connecting piece for semiconductor device and preparation method of connecting piece
The nanostructured array and graphene layer were prepared by femtosecond laser, and the hot-press welding connection was combined with nano silver paste, which solved the shortcomings of traditional packaging materials under high temperature conditions, achieved low-temperature sintering and high-temperature stability improvement, and was suitable for high-power semiconductors Microelectronic package interconnection of devices.
Patent Information
- Application Number
- CN202411055597.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional packaging connection materials cannot meet the needs of high-power semiconductor devices under high temperature conditions, resulting in excessive sintering temperature and large residual stress, which damages the chip and packaging system.
Femtosecond laser is used to prepare nanostructured arrays and graphene layers, and combined with nanosilver paste for hot-press welding connections to reduce the sintering temperature and improve the shear strength and oxidation resistance of the connection interface.
Low-temperature sintering is achieved, internal stress is reduced, semiconductor device life is extended, high-temperature stability is improved, and semiconductor device normal operation in extreme environments.
Smart Images

Figure CN118983289A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of microelectronics technology, and in particular to a connector for a semiconductor device and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, high-power semiconductor devices that can withstand working conditions above 200°C have received widespread attention. Reliable interconnection technology provides mechanical support and electrical interconnection for semiconductor chips. Since high-power semiconductor devices can serve under high temperature conditions, the corresponding packaging connection materials and packaging connection interfaces must also be able to serve under high temperature conditions, but traditional packaging connection materials cannot meet this requirement. During the connection process of traditional solder, the connection temperature must exceed the melting point of the solder, which will not only produce high residual stress, but may even directly damage the chip and packaging system. Therefore, new packaging materials and packaging processes are needed. Summary of the invention
[0003] The purpose of the present application is to provide a connector for semiconductor devices and a preparation method thereof, which can reduce the sintering temperature, improve the shear strength of the connection interface, enhance the oxidation resistance, have good high-temperature stability, help to ensure the normal operation of high-power semiconductor devices in various extreme environments, and have broad application prospects in the field of microelectronic packaging interconnection.
[0004] The technical solution of this application is as follows:
[0005] The embodiment of the present application provides a connector for a semiconductor device, which includes two conductive substrates arranged opposite to each other, and a sealing layer connected between the two conductive substrates;
[0006] A nanostructure array is disposed on a surface of any of the conductive substrates close to the sealing layer;
[0007] The transverse cross section of the nanostructure array is in a grid shape, the longitudinal cross section of the nanostructure array is in a sawtooth shape, and a single structural unit of the nanostructure array is in a pyramid shape;
[0008] A graphene layer is disposed on the surface of any one of the nanostructure arrays, and the sealing layer is disposed between two of the graphene layers.
[0009] Furthermore, in some embodiments of the present application, the conductive substrate is a copper substrate; and the material of the sealing layer is nano silver paste.
[0010] The present application also provides a method for preparing the above-mentioned connector for semiconductor devices, which comprises the following steps:
[0011] a: ultrasonically clean the conductive substrate in anhydrous ethanol to remove surface impurities;
[0012] b: The nanostructure array is processed on the surface of the conductive substrate by means of a femtosecond laser, and then ultrasonically cleaned and dried in anhydrous ethanol;
[0013] c: Preparation of graphene layer on the surface of nanostructure array;
[0014] d: Using hot pressing welding, two conductive substrates processed with nanostructure arrays and graphene layers are sintered and connected through nano silver paste to obtain a finished connector.
[0015] Further, in some embodiments of the present application, in the above step b, the conductive substrate is placed on a three-dimensional motion platform, the three-dimensional motion platform moves according to a set path, and a femtosecond laser is used to ablate the surface of the conductive substrate according to the path to prepare a nanostructure array;
[0016] Among them, the three-dimensional motion platform moves according to continuous longitudinal S-shaped and continuous transverse S-shaped paths respectively.
[0017] Furthermore, in some embodiments of the present application, in the above step b, the working conditions of the femtosecond laser are: power 700mw, central wavelength 1030nm, repetition frequency 75kHz, pulse duration 215fs, scanning speed 2000mm / s, and scanning spacing 5μm.
[0018] Further, in some embodiments of the present application, in the above step c, the method for preparing the graphene layer is:
[0019] Prepare an EVA solution and a copper-based monolayer graphene, drop the EVA solution, spin-coat it on the surface of the copper-based monolayer graphene, and then dry it to form an EVA solid film on the surface of the copper-based monolayer graphene, so as to obtain a three-layer structure material having a copper foil substrate, a graphene layer, and an EVA film in sequence;
[0020] The three-layer structure material is immersed in an ammonium persulfate solution, and the copper foil substrate is etched away to obtain a double-layer structure material having an EVA film and a graphene layer, and then washed with deionized water;
[0021] The double-layer structure material is transferred to the surface of the conductive substrate, the graphene layer is brought into contact with the nanostructure array, and the double-layer structure material is heated and dried so as to be tightly combined with the surface of the conductive substrate to obtain a sample;
[0022] The sample was placed in a xylene solution and heated to remove the EVA film, leaving the graphene layer on the surface of the nanostructure array, thereby obtaining a conductive substrate covered with a single layer of graphene.
[0023] Furthermore, in some embodiments of the present application, in the above step c, the EVA solution is a xylene solution of 40 wt % vinyl acetate, and the mass fraction of vinyl acetate in the solution is 10%; the concentration of the ammonium persulfate solution used is 3 wt %.
[0024] Furthermore, in some embodiments of the present application, in the above step c, in the process of preparing the above three-layer structure material, the EVA solution is dropped on the surface of the copper-based monolayer graphene, and the EVA solution is evenly coated on the surface of the copper-based monolayer graphene by a spin coater at a rate of 4000r / min for 60s, and then dried.
[0025] Furthermore, in some embodiments of the present application, in the above step c, in the process of preparing the above three-layer structure material, the EVA solution is dripped and spin-coated on the surface of the copper-based single-layer graphene, and then dried at 80° C. for 60 minutes.
[0026] Furthermore, in some embodiments of the present application, in the above step c, during the process of preparing the sample, the double-layer structure material is transferred to the surface of the conductive substrate so that the graphene layer is in contact with the nanostructure array, and dried at 80° C. for 3 hours.
[0027] Furthermore, in some embodiments of the present application, in the above step c, in the process of preparing the conductive substrate covered with a single layer of graphene, the sample is placed in a xylene solution, heated to 80° C. in a water bath and kept warm for 30 minutes, and the EVA film is removed.
[0028] Furthermore, in some embodiments of the present application, in the above step d, when sintering connection is performed by means of hot pressing welding, the process conditions are: applying a pressure of 0 to 10 MPa, a sintering temperature of 180 to 300° C., and a sintering time of 10 to 60 min.
[0029] Furthermore, in some embodiments of the present application, in the above step d, the ingredients of the nano silver paste used are: nano silver powder, polyethylene glycol, glycerol and diethylene glycol butyl ether acetate.
[0030] Furthermore, in some embodiments of the present application, in the above step d, the particle size of the nano silver powder used in the nano silver paste is 20 nm.
[0031] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects:
[0032] The embodiment of the present application provides a connector for semiconductor devices and a preparation method thereof; femtosecond laser has the advantages of extremely short pulse duration, extremely high pulse peak power, and three-dimensional ultra-precision. It uses femtosecond laser to prepare a nanostructure array on the surface of a conductive substrate, which can reduce the sintering temperature while ensuring a high connection strength, achieve the goal of "low temperature sintering" of the interconnection structure, reduce the internal stress of the interconnection system, and thus extend the service life of the semiconductor device. By preparing a layer of graphene on the surface of the nanostructure array, the generation of interface oxides under high-temperature working environment can be effectively suppressed, and the generation of cracks in the connection interface can be prevented, thereby improving the high-temperature stability of the device and achieving the goal of "high-temperature service" of the semiconductor device. The entire connector structure is complete and simple, with stable performance and easy preparation, which helps to ensure the normal operation of high-power semiconductor devices in various extreme environments. It has broad application prospects in the field of microelectronic packaging interconnection and is conducive to actual production and promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 A schematic diagram of the motion path of the three-dimensional motion platform in the process of preparing the nanostructure array in the embodiment of the present application;
[0035] Figure 2 This is a schematic diagram of a process flow for preparing a connector for a semiconductor device in an embodiment of the present application;
[0036] Figure 3 This is a comparison chart of the shear strength of the products of Comparative Example 1 and Example 1 of the present application;
[0037] Figure 4 This is a performance comparison chart of the products of comparative example 2 and embodiment 2 of the present application.
[0038] Figure numerals: 1 - conductive substrate, 2 - nanostructure array, 3 - graphene layer, 4 - sealing layer. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] In the description of the embodiments of the present application, it should be noted that if the terms "longitudinal", "lateral", etc. appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the accompanying drawings, or is the orientation or position relationship in which the product of the application is usually placed when used. It is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0041] It should be noted that the term "include" or any other variation thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "include..." do not exclude the existence of other identical elements in the process, method, article or device including its elements.
[0042] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.
[0043] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0044] Example 1
[0045] See also Figure 1-2 , the embodiment of the present application provides a connector for a semiconductor device, which is prepared by the following method:
[0046] a: prepare two copper conductive substrates 1 (the conductive substrate 1 at the lower layer has a size of 12 mm×12 mm×1 mm, and the conductive substrate 1 at the upper layer has a size of 3 mm×3 mm×1 mm), and ultrasonically clean the conductive substrates 1 in anhydrous ethanol for 5 minutes to remove surface impurities;
[0047] b: Place the conductive substrate 1 on a three-dimensional motion platform. The three-dimensional motion platform is moved as follows: Figure 1 The path shown is continuously longitudinally S-shaped and horizontally S-shaped, and the surface of the conductive substrate 1 is ablated along the path using a femtosecond laser to prepare a nanostructure array 2;
[0048] The working conditions of the femtosecond laser are: power 700mw, central wavelength 1030nm, repetition frequency 75kHz, pulse duration 215fs, scanning speed 2000mm / s, and scanning spacing 5μm.
[0049] After processing, it was ultrasonically cleaned in anhydrous ethanol for 10 minutes and dried to remove impurities such as debris and oxides generated during processing;
[0050] c: Preparing a graphene layer 3 on the surface of the nanostructure array 2, the specific method is:
[0051] Prepare an EVA solution and a copper-based monolayer graphene, drop the EVA solution on the surface of the copper-based monolayer graphene, spin coat the EVA solution at a rate of 4000 r / min for 60 seconds using a spin coater to evenly coat the surface of the copper-based monolayer graphene, and then dry the solution at 80° C. for 60 minutes to form an EVA solid film on the surface of the copper-based monolayer graphene, thereby obtaining a three-layer structure material having a copper foil substrate, a graphene layer 3, and an EVA film in sequence;
[0052] Wherein, the EVA solution is a xylene solution of 40wt% vinyl acetate, and the mass fraction of vinyl acetate in the solution is 10%;
[0053] The three-layer structure material is immersed in a 3wt% ammonium persulfate solution for 5 hours, and the copper foil substrate is etched away to obtain a double-layer structure material having an EVA film and a graphene layer 3, and then washed with deionized water;
[0054] The double-layer structure material is transferred to the surface of the conductive substrate 1, so that the graphene layer 3 is in contact with the nanostructure array 2 and heated to 80° C. and dried for 3 hours, so that the double-layer structure material is tightly combined with the surface of the conductive substrate 1 to obtain a sample;
[0055] The sample was placed in a xylene solution, heated to 80° C. in a water bath and kept warm for 30 min, and the EVA film was removed, leaving the graphene layer 3 on the surface of the nanostructure array 2 to obtain a conductive substrate 1 covered with a single layer of graphene.
[0056] d: Using hot pressing welding, two conductive substrates 1 processed with nanostructure arrays 2 and graphene layers 3 are sintered and connected through nano silver paste. The sintering conditions are: applying a pressure of 0 to 10 MPa, a sintering temperature of 180 to 300° C., and a sintering time of 10 to 60 min.
[0057] The composition of the nano silver paste is: 80wt% of nano silver powder with a particle size of 20nm, 16wt% of polyethylene glycol, 2wt% of propylene glycol, and 2wt% of diethylene glycol butyl ether acetate;
[0058] After sintering, the nano silver paste forms a sealing layer 4 to obtain a finished connector.
[0059] Comparative Example 1
[0060] This comparative example is based on Example 1, and differs from Example 1 in that the nanostructure array 2 is not prepared on the surface of the conductive substrate 1, and the graphene layer 3 is directly prepared and the subsequent steps are continued. The relevant process conditions and parameters are the same as those in Example 1.
[0061] Comparison of shear strength of the connector obtained in Comparative Example 1 and Example 1 Figure 3 shown.
[0062] Depend on Figure 3 It can be seen that the shear strength of the nanostructure array 2 is higher, indicating that the nanostructure array 2 can be well embedded in the sintered packaging layer, so that the connection interface between the conductive substrate 1 and the packaging layer forms a mechanical interlocking, thereby improving its strength performance.
[0063] Comparative Example 2
[0064] This comparative example is based on Example 1, and differs from Example 1 in that the graphene layer 3 is not prepared, and the remaining steps are the same as those of Example 1, and the relevant process condition parameters are the same as those of Example 1.
[0065] Comparison of the performance of the connector obtained in Comparative Example 2 and Example 1 Figure 4 shown.
[0066] Depend on Figure 4 It can be seen that by preparing a single layer of graphene covering the surface of the nanostructure array 2, the generation of oxides can be effectively inhibited. After aging at a high temperature of 300°C for 48 hours, the thickness of the oxide generated by the connector product with the graphene layer 3 is about 1 / 3 of that of the connector product without the graphene layer 3, and the shear strength is also higher.
[0067] It shows that by preparing the graphene layer 3, the connection interface between the conductive substrate 1 and the packaging layer can be effectively prevented from oxidative fracture, thereby improving the high-temperature stability of the connection structure. In addition, graphene has excellent conductive properties and will not affect the electrical properties of the interconnection structure.
[0068] In summary, the embodiment of the present application provides a connector for semiconductor devices and a preparation method thereof, which uses a femtosecond laser to prepare a nanostructure array 2 on the surface of a conductive substrate 1, which can reduce the sintering temperature while ensuring a high connection strength, achieve the goal of "low temperature sintering" of the interconnection structure, reduce the internal stress of the interconnection system, and thus extend the service life of the semiconductor device. By preparing a layer of graphene on the surface of the nanostructure array 2, the generation of interface oxides in a high-temperature working environment can be effectively suppressed, and the generation of cracks in the connection interface can be prevented, thereby improving the high-temperature stability of the device and achieving the goal of "high-temperature service" of the semiconductor device. The entire connector has a complete and simple structure, stable performance, and is easy to prepare. It helps to ensure the normal operation of high-power semiconductor devices in various extreme environments. It has broad application prospects in the field of microelectronic packaging interconnection and is conducive to actual production and promotion.
[0069] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
Claims
1. A connector for a semiconductor device, characterized in that: It includes two conductive substrates arranged opposite to each other, and a sealing layer connected between the two conductive substrates; A nanostructure array is disposed on a surface of any one of the conductive substrates close to the sealing layer; The transverse cross section of the nanostructure array is in a grid shape, the longitudinal cross section of the nanostructure array is in a sawtooth shape, and a single structural unit of the nanostructure array is in a pyramid shape; A graphene layer is disposed on the surface of any one of the nanostructure arrays, and the sealing layer is disposed between two of the graphene layers.
2. A connector for a semiconductor device according to claim 1, characterized in that: The conductive substrate is a copper substrate; the material of the sealing layer is nano silver paste.
3. A method for preparing a connector for a semiconductor device according to any one of claims 1 to 2, characterized in that: It includes the following steps: a: ultrasonically clean the conductive substrate in anhydrous ethanol to remove surface impurities; b: The nanostructure array is processed on the surface of the conductive substrate by means of a femtosecond laser, and then ultrasonically cleaned and dried in anhydrous ethanol; c: Preparation of graphene layer on the surface of nanostructure array; d: Using hot pressing welding, two conductive substrates processed with nanostructure arrays and graphene layers are sintered and connected through nano silver paste to obtain a finished connector.
4. The method for preparing a connector for a semiconductor device according to claim 3, characterized in that: In the step b, the conductive substrate is placed on a three-dimensional motion platform, the three-dimensional motion platform moves according to a set path, and a femtosecond laser is used to ablate the surface of the conductive substrate according to the path to prepare a nanostructure array; Among them, the three-dimensional motion platform moves according to continuous longitudinal S-shaped and continuous transverse S-shaped paths respectively.
5. The method for preparing a connector for a semiconductor device according to claim 3, characterized in that: In the step b, the working conditions of the femtosecond laser are: power 700mw, central wavelength 1030nm, repetition frequency 75kHz, pulse duration 215fs, scanning speed 2000mm / s, and scanning interval 5μm.
6. The method for preparing a connector for a semiconductor device according to claim 3, characterized in that: In the step c, the method for preparing the graphene layer is: Prepare an EVA solution and a copper-based monolayer graphene, drop the EVA solution, spin-coat it on the surface of the copper-based monolayer graphene, and then dry it to form an EVA solid film on the surface of the copper-based monolayer graphene, so as to obtain a three-layer structure material having a copper foil substrate, a graphene layer, and an EVA film in sequence; The three-layer structure material is immersed in an ammonium persulfate solution, and the copper foil substrate is etched away to obtain a double-layer structure material having an EVA film and a graphene layer, and then washed with deionized water; The double-layer structure material is transferred to the surface of the conductive substrate, the graphene layer is brought into contact with the nanostructure array, and the double-layer structure material is heated and dried so as to be tightly combined with the surface of the conductive substrate to obtain a sample; The sample was placed in a xylene solution and heated to remove the EVA film, leaving the graphene layer on the surface of the nanostructure array, thereby obtaining a conductive substrate covered with a single layer of graphene.
7. The method for preparing a connector for a semiconductor device according to claim 6, characterized in that: In the step c, the EVA solution is a xylene solution of 40 wt % vinyl acetate, the mass fraction of vinyl acetate in the solution is 10%; the concentration of the ammonium persulfate solution used is 3 wt %.
8. The method for preparing a connector for a semiconductor device according to claim 3, characterized in that: In the step d, when the sintering connection is performed by means of hot pressing welding, the process conditions are: applying a pressure of 0 to 10 MPa, a sintering temperature of 180 to 300° C., and a sintering time of 10 to 60 min.
9. The method for preparing a connector for a semiconductor device according to claim 3, characterized in that: In the step d, the nano silver paste used comprises the following ingredients: nano silver powder, polyethylene glycol, glycerol and diethylene glycol butyl ether acetate.
10. The method for preparing a connector for a semiconductor device according to claim 9, characterized in that: In the step d, the particle size of the nano silver powder used in the nano silver paste is 20 nm.
Citation Information
Patent Citations
Copper interconnection functional microstructure and preparation method thereof
CN109473418A