Test structure, failure positioning method and failure analysis method

By designing a test structure containing comb-shaped structure and metal wires, the failure points are quickly positioned using the light and dark differences in the voltage contrast image, the problem of inaccurate positioning and easy to miss small-size defects in the existing technology is solved, and the failure positioning is improved and the efficiency and accuracy of the analysis.

CN118983302APending Publication Date: 2024-11-19SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411037930.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art cannot accurately locate the failure points through SEM VC observation, resulting in the need to conduct large-scale searches in hot spot areas, which is time-consuming and labor-intensive and easy to miss small-sized structures.

Method used

A test structure is designed, including a comb structure, a metal connection and a plurality of semiconductor structures. The active region and gate in the semiconductor structure are connected in sequence through metal connections, so that light and dark differences occur in the voltage contrast image, thereby Quickly locate the failure points.

Benefits of technology

Improves the efficiency and accuracy of failure positioning, reduces the risk of omission of small-size defects, and simplifies the analysis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983302A_ABST
    Figure CN118983302A_ABST
Patent Text Reader

Abstract

The invention provides a test structure, a failure positioning method and a failure analysis method. The test structure comprises a comb-shaped structure, a metal connecting wire and a plurality of semiconductor structures, the semiconductor structure comprises a well region, an active region and a plurality of grid electrodes, and the grid electrodes are arranged at intervals in the first direction. In two adjacent semiconductor structures, the active region and the plurality of grids in one semiconductor structure are connected in sequence through metal connecting lines; the active region and the plurality of grids in the other semiconductor structure are connected with the metal connecting wires in a one-to-one correspondence manner, and the metal connecting wires in one-to-one correspondence are mutually independent; and the comb-shaped structure is connected with the semiconductor structure through a metal connecting wire. According to the configuration, the two different metal connecting wires are arranged at intervals in the connecting mode, so that the brightness difference can be seen in a voltage contrast image, abnormal failure points can be quickly positioned, the failure positioning efficiency is improved, meanwhile, small-size defects are not prone to being omitted, and the failure positioning accuracy is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a test structure, a failure location method and a failure analysis method. Background Art

[0002] In the process of developing advanced semiconductor processes, various test structures are designed to detect process problems on the line to reflect the problems existing in the current process. For example, the test structure used to monitor the metal gate cutting process, the metal gate is connected to the first metal comb structure and the second metal comb structure respectively (see Figure 1 ), by detecting whether the electrical properties of the first metal comb structure and the second metal comb structure are short-circuited to monitor whether the metal gate is bridged, so as to monitor the quality of the metal gate cutting process. If the inner layer of the strip is short-circuited, the short-circuit position needs to be located for further TEM (Transmission Electron Microscope) morphology analysis.

[0003] For the failed structure with short circuit, it will first be located through OBIRCH (Optical Beam Induced Resistance Change) / EBIRCH (Electron Beam Induced Resistance Change), and then the hot spot will be observed by SEM VC (Scanning Electron Microscope; Voltage-Contrast) and SEM HV (Scanning Electron Microscope; Higlt-Voltage) to locate the failure point. However, since the metal gate is a floating gate structure, if a short circuit occurs between them, the failed metal gate and the normal metal gate will appear gray in the voltage contrast image, and the failure position cannot be further accurately located. It can only be located by SEM HV observation of the hot spot area. This method is time-consuming and labor-intensive, and it is easy to miss defects in small-size structures, resulting in inaccurate positioning and inability to effectively analyze the cause of failure. Summary of the invention

[0004] The purpose of the present invention is to provide a test structure, a failure location method and a failure analysis method to solve the problem in the prior art that the failure point cannot be accurately located by SEM VC observation, so that a large-scale search is required in the hot spot area, which is time-consuming and labor-intensive and easily misses defects of small-sized structures.

[0005] In order to achieve the above object, the present invention provides a test structure, including: a comb structure, a metal connection and a plurality of semiconductor structures;

[0006] The semiconductor structure comprises: a well region, an active region and a plurality of gates disposed on the well region, wherein the plurality of gates are arranged at intervals along a first direction;

[0007] The plurality of semiconductor structures are arranged at intervals along the second direction. In two adjacent semiconductor structures, the active region and the plurality of gates in one semiconductor structure are sequentially connected through one metal wire; the active region and the plurality of gates in the other semiconductor structure are connected to the metal wire in a one-to-one correspondence, and the one-to-one corresponding metal wires are independent of each other.

[0008] The comb-shaped structure is connected to the semiconductor structure through the metal wiring.

[0009] Optionally, the test structure includes a first interconnect structure and a second interconnect structure;

[0010] The first interconnect structure is formed by sequentially connecting the active region and the plurality of gates in one of the semiconductor structures with the metal wires;

[0011] The second interconnect structure is formed by connecting the metal wires with the active region and the plurality of gates in one semiconductor structure in a one-to-one correspondence;

[0012] The first interconnect structures and the second interconnect structures are alternately arranged along the second direction.

[0013] Optionally, the test structure includes a first through hole and two comb-like structures, the first through hole is arranged in one-to-one correspondence with the gate, and the two comb-like structures are respectively connected to the first interconnection structure and the second interconnection structure through the first through hole.

[0014] Optionally, the comb-like structure includes a comb back and a plurality of comb teeth, the comb teeth extend along the first direction, the plurality of comb teeth are arranged at intervals along the second direction, and the comb back is sequentially connected to one end of the plurality of comb teeth;

[0015] The comb teeth of one of the comb-like structures are connected to the first interconnection structures in a one-to-one correspondence; the comb teeth of the other comb-like structure are connected to the second interconnection structures in a one-to-one correspondence.

[0016] Optionally, the comb-like structure further includes a second through hole, which is arranged on one side of the comb teeth, and the comb teeth are connected to the comb back through the second through hole, and the second through holes in the same comb-like structure are located on the same side of the comb teeth.

[0017] Optionally, the comb teeth include a first metal layer; and the comb back includes a second metal layer.

[0018] Optionally, the first direction and the second direction are perpendicular to each other.

[0019] In order to achieve the above object, the present invention further provides a failure location method, comprising:

[0020] Providing a sample including the test structure as described above, wherein the sample includes a failure point;

[0021] Obtaining a hot spot area of ​​the sample, wherein the failure point is located in the hot spot area;

[0022] Grinding the sample to the first through-hole layer, and performing voltage contrast observation on the sample to obtain a voltage contrast image;

[0023] The voltage contrast image is observed to compare the brightness difference of the first through hole to locate the failure point.

[0024] Optionally, the sample includes a first interconnect structure and a second interconnect structure;

[0025] The first through hole located above the first interconnect structure is in a highlighted state in the voltage contrast image; the first through hole located above the second interconnect structure is in a dark state in the voltage contrast image;

[0026] The step of observing the voltage contrast image and comparing the light and dark difference of the first through hole to locate the failure point comprises:

[0027] If the first through hole located above the second interconnect structure is highlighted in the voltage contrast image, the failure point is a position corresponding to the first through hole in the second interconnect structure.

[0028] In order to achieve the above object, the present invention also provides a failure analysis method, comprising:

[0029] Using the failure location method as described above, the failure point of the sample is located;

[0030] Performing accelerated voltage observation on the failure point by SEM; or,

[0031] TEM samples were prepared and observed to analyze the failure mechanism.

[0032] Compared with the prior art, the test structure, failure location method and failure location method provided by the present application have the following advantages:

[0033] The test structure provided in the present application sequentially connects an active area and multiple gates in a semiconductor structure through metal wiring, so that in a voltage contrast image, a first through hole located above the corresponding semiconductor structure is highlighted, while in another semiconductor structure adjacent thereto, the metal wiring is connected to the active area and multiple gates in a one-to-one correspondence, and in the voltage contrast image, the first through hole located above the corresponding semiconductor structure is dark. Therefore, by arranging the connection methods of the above two different metal wirings at intervals, the difference in brightness can be seen in the voltage contrast image, and the abnormal failure point can be quickly located, thereby improving the efficiency of failure location, and at the same time, it is not easy to miss small-size defects, further improving the accuracy of failure location.

[0034] The failure location method provided in the present application, by using the above-mentioned test structure, allows the operator to search for the first through hole with abnormal light and dark states in the voltage contrast image only to determine that the corresponding position in the semiconductor structure below the first through hole is the failure point. It is no longer necessary to search over a large area in the hot spot area, which improves the efficiency of failure analysis while making it less likely to miss small-sized defects, further improving the accuracy of failure analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a schematic diagram of a test structure in the prior art;

[0036] Figure 2 A voltage contrast image of a test structure in the prior art;

[0037] Figure 3 A schematic diagram of a test structure provided by an embodiment of the present invention;

[0038] Figure 4 A cross-sectional view of a test structure provided by an embodiment of the present invention;

[0039] Figure 5 A voltage contrast image of a test structure provided by an embodiment of the present invention;

[0040] Figure 6 A flowchart of a failure location method provided by an embodiment of the present invention;

[0041] Figure 7 A flowchart of a failure analysis method provided by an embodiment of the present invention;

[0042] The description of each reference numeral is as follows:

[0043] 10-semiconductor structure; 100-well region; 101-gate;

[0044] 11-Metal connection;

[0045] 12-comb-like structure; 120-comb teeth; 121-comb back; 122-first metal layer; 123-second metal layer; 124-second through hole;

[0046] 13-first through hole; 14-soldering pad;

[0047] 20-first metal comb structure; 21-second metal comb structure; 22-metal gate; 23-connecting line;

[0048] X-first direction; Y-second direction. DETAILED DESCRIPTION

[0049] In order to make the purpose, advantages and features of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and are not drawn to scale, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In addition, the structure shown in the drawings is often a part of the actual structure. In particular, the emphasis of each drawing is different, and sometimes different scales are used.

[0050] As used in this specification, the singular forms "a", "an" and "the" include plural objects, the term "or" is generally used to include the meaning of "and / or", the term "several" is generally used to include the meaning of "at least one", and the term "at least two" is generally used to include the meaning of "two or more". In addition, the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second" and "third" may explicitly or implicitly include one or at least two of the features, "one end" and "the other end" and "the proximal end" and "the distal end" generally refer to two corresponding parts, which include not only the endpoints, and the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral body; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. In addition, as used in this specification, an element disposed on another element generally only indicates that there is a connection, coupling, cooperation or transmission relationship between the two elements, and the connection, coupling, cooperation or transmission between the two elements may be direct or indirect through an intermediate element, and it cannot be understood as indicating or implying the spatial position relationship between the two elements, that is, one element may be in any orientation such as inside, outside, above, below or on one side of another element, unless the content clearly indicates otherwise. The terms "upper", "lower", "top" and "bottom" are generally relative position relationships arranged in the direction of gravity; the terms "vertical, vertical direction" generally refer to the direction of gravity, which is generally perpendicular to the ground, and "horizontal, horizontal plane direction" generally refers to the direction parallel to the ground; for ordinary technicians in this field, the specific meanings of the above terms in this specification can be understood according to specific circumstances.

[0051] The purpose of the present invention is to provide a test structure, a failure location method and a failure analysis method to solve the problem in the prior art that the failure point cannot be accurately located by SEM VC observation, so that a large-scale search is required in the hot spot area, which is time-consuming and labor-intensive and easily misses defects of small-sized structures.

[0052] Please refer to Figure 1 and Figure 2 , those skilled in the art can understand that, Figure 1The test structure shown is used to monitor the metal gate 22 cutting process. The test structure includes a first metal comb structure 20, a second metal comb structure 21, and a plurality of metal gates 22 and an active area arranged on the well area. The metal gate 22 and the active area are respectively connected to the first metal comb structure 20 and the second metal comb structure 21 through connecting wires 23, and the connecting wires 23 are connected to the plurality of metal gates 22 and the active area one by one, and the plurality of connecting wires 23 are independent of each other. Whether the metal gate 22 is bridged (Bridge) is monitored by detecting whether the electrical properties of the first metal comb structure 20 and the second metal comb structure 21 are short-circuited. However, in the failure location process, since the metal gate 22 is a floating gate structure, the metal gate 22 presents a consistent state in the voltage contrast image (such as Figure 2 As shown in the figure, the failure point cannot be accurately located and can only be located by SEM HV observation of the hot spot area, which reduces the efficiency of failure location and easily misses small defects, reducing the accuracy of failure location.

[0053] Based on this, please refer to Figures 3 to 5The present invention provides a test structure, comprising: a comb structure 12, a metal connection 11 and a plurality of semiconductor structures 10; the semiconductor structure 10 comprises: a well region 100, an active region and a plurality of gates 101 arranged on the well region 100, and the plurality of gates 101 are arranged at intervals along a first direction X; the plurality of semiconductor structures 10 are arranged at intervals along a second direction Y, and in two adjacent semiconductor structures 10, the active region and the plurality of gates 101 in one semiconductor structure 10 are sequentially connected through a metal connection 11; the active region and the plurality of gates 101 in another semiconductor structure 10 are connected to the metal connection 11 in a one-to-one correspondence, and the one-to-one corresponding metal connections 11 are independent of each other; the comb structure 12 is connected to the semiconductor structure 10 through the metal connection 11. In an optional embodiment, the first direction X and the second direction Y are perpendicular to each other. In some other embodiments, the first direction X and the second direction Y may also be arranged at other angles, and those skilled in the art may configure this according to actual conditions. It should be noted that in two semiconductor structures 10 adjacent to each other along the second direction Y, the metal connection 11 is provided with two different connection modes. One is to use a metal connection 11 to connect the active area and all gates 101 in a semiconductor structure 10 (that is, to connect m0a and m0p together, wherein m0a is the metal zero layer of the active area, which is used to achieve the contact between the wire and the active area; m0p is the metal zero layer connected to the gate 101, which is used to achieve the contact between the wire and the gate 101 structure). This connection mode is equivalent to grounding the semiconductor structure 10. , so in the voltage contrast image, the first through hole 13 located above the semiconductor structure 10 will appear in a highlighted state; the other is the same as the prior art, connecting multiple metal wires 11 to the active area and multiple gates 101 in another semiconductor structure 10 in a one-to-one correspondence, and adjacent metal wires 11 are directly independent of each other (i.e., m0a and m0p are independently set), this connection method is equivalent to the semiconductor structure 10 not being grounded, so in the voltage contrast image, the first through hole 13 located above the semiconductor structure 10 will appear in a dark state. After obtaining the hot spot area, the operator can perform SEM VC (scanning electron microscope voltage contrast) observation in the hot spot area, so as to accurately locate the position where the light and dark state is abnormal, and thus successfully locate the failure point.

[0054] With this configuration, Figure 1Compared with the test structure shown, the active area and multiple gates 101 in a semiconductor structure 10 are connected in sequence through the metal connection 11, so that in the voltage contrast image, the first through hole 13 located above the corresponding semiconductor structure 10 is highlighted, while the active area and the gate 101 are connected by the existing connection method. In the voltage contrast image, the first through hole 13 located above the corresponding semiconductor structure 10 is dark. Therefore, by arranging the connection methods of the above two different metal connections 11 at intervals, the difference in light and dark can be seen in the voltage contrast image, and the abnormal failure point can be quickly located, which improves the efficiency of failure location, and is not easy to miss small-size defects, further improving the accuracy of failure location.

[0055] As an alternative embodiment, please refer to Figures 2 to 5 The test structure includes a first interconnection structure and a second interconnection structure; the first interconnection structure is formed by metal wires 11 sequentially connecting an active region in a semiconductor structure 10 and multiple gates 101; the second interconnection structure is formed by metal wires 11 and active regions in a semiconductor structure 10 and multiple gates 101 correspondingly connected one by one; the first interconnection structure and the second interconnection structure are alternately arranged along the second direction Y. It should be noted that the first interconnection structure is as follows Figure 4 and Figure 5 As shown, a metal wire 11 connects an active region and all gates 101 in a semiconductor structure 10. The second interconnect structure is as shown in FIG. Figure 2 As shown, a plurality of metal wires 11 are connected one by one to an active region and a gate 101 in a semiconductor structure 10; please refer to Figure 3 , the first interconnection structure and the second interconnection structure are alternately arranged along the second direction Y, that is, among the multiple semiconductor structures 10 arranged at intervals along the second direction Y, the odd-numbered or even-numbered semiconductor structures 10 are connected to the metal wiring 11 to form the first interconnection structure, and the remaining semiconductor structures 10 are connected to the metal wiring 11 to form the second interconnection structure. In other embodiments, the arrangement of the first interconnection structure and the second interconnection structure may also be in other forms, as long as it is ensured that any one of the two adjacent semiconductor structures 10 is the first interconnection structure and the other is the second interconnection structure.

[0056] Please refer to Figure 3, the test structure includes a first through hole 13 and two comb-like structures 12, the first through hole 13 is arranged in a one-to-one correspondence with the gate 101, and the two comb-like structures 12 are respectively connected to the first interconnection structure and the second interconnection structure through the first through hole 13. Further, the comb-like structure 12 includes a comb back 121 and a plurality of comb teeth 120, the comb teeth 120 extend along the first direction X, and the plurality of comb teeth 120 are arranged at intervals along the second direction Y, and the comb back 121 is sequentially connected to one end of the plurality of comb teeth 120; the comb teeth 120 of one of the comb-like structures 12 are respectively connected to the first interconnection structure in a one-to-one correspondence; the comb teeth 120 of the other comb structure 12 are respectively connected to the second interconnection structure in a one-to-one correspondence. It should be noted that in Figure 3 In the illustrated example, the comb back 121 extends along the second direction Y and is respectively connected to one end of the plurality of comb teeth 120 along the first direction X. The comb teeth 120 are provided with a plurality of first through holes 13 spaced along the second direction Y, and the position of each first through hole 13 matches the position of the gate 101 in the semiconductor structure 10, so that in the subsequent failure location process, the location can be quickly achieved through the light and dark state of the first through hole 13. At the same time, a pad 14 is also led out at one end of the comb back 121 to facilitate electrical testing of the test structure.

[0057] As an optional embodiment, please continue to refer to Figure 3 , the comb-like structure 12 also includes a second through hole 124, which is arranged on one side of the comb teeth 120, and the comb teeth 120 are connected to the comb back 121 through the second through hole 124, and the second through hole 124 in the same comb-like structure 12 is located on the same side of the comb teeth 120. Further, the comb teeth 120 include a first metal layer 122; the comb back 121 includes a second metal layer 123. It should be noted that the first metal layer 122 and the second metal layer 123 can both be metal connecting wires. In this embodiment, the comb teeth 120 and the comb back 121 are arranged at different levels. In other embodiments, the comb teeth 120 and the comb back 121 can also be arranged at the same level. Those skilled in the art can configure this according to actual conditions. At the same time, the second through hole 124 in the same comb-like structure 12 is located on the same side of the comb teeth 120, which facilitates the connection between the comb back 121 and the comb teeth 120.

[0058] Please refer to Figure 6 In another embodiment, the present invention further provides a failure location method, comprising:

[0059] Step S1: providing a sample including the test structure as described above, wherein the sample includes a failure point;

[0060] Step S2: obtaining a hot spot area of ​​the sample, wherein the failure point is located in the hot spot area;

[0061] Step S3: grinding the sample to the first through hole 13 layer, and performing voltage contrast observation on the sample to obtain a voltage contrast image;

[0062] Step S4: By observing the voltage contrast image, the light and dark differences of the first through hole 13 are compared to locate the failure point.

[0063] It should be noted that in step S1, positioning is performed by OBIRCH (Optical Beam Induced Resistance Change) or EBIRCH (Electron Beam Induced Resistance Change) to obtain the hot spot area of ​​the sample; in step S3, voltage contrast observation of the sample is performed by SEM (Scanning Electron Microscope). By using the above-mentioned test structure, the operator only needs to search for the first through hole 13 with abnormal light and dark states in the voltage contrast image to determine that the corresponding position in the semiconductor structure 10 below the first through hole 13 is the failure point, and it is no longer necessary to search in a large range in the hot spot area, which improves the efficiency of failure analysis while not easily missing small-sized defects, further improving the accuracy of failure analysis.

[0064] Further, the sample includes a first interconnection structure and a second interconnection structure; the first through hole 13 located above the first interconnection structure is in a highlighted state in the voltage contrast image; the first through hole 13 located above the second interconnection structure is in a dark state in the voltage contrast image;

[0065] By observing the voltage contrast image and comparing the light and dark differences of the first through hole 13, the failure point can be located, including:

[0066] Step S41: If the first through hole 13 located above the second interconnect structure is in a highlighted state in the voltage contrast image, the failure point is the position corresponding to the first through hole 13 in the second interconnect structure.

[0067] It should be noted that in the present embodiment, by adopting different connection modes of the metal wires 11, the first through hole 13 above the first interconnection structure appears in a highlighted state in the voltage contrast image, and the first through hole 13 above the second interconnection structure appears in a dark state in the voltage contrast image. In other embodiments, other forms may be used to make two adjacent interconnection structures appear different in brightness in the voltage contrast image, and the present embodiment does not impose any limitation on this.

[0068] Please refer to Figure 7 In another embodiment, the present invention further provides a failure analysis method, comprising:

[0069] Step S10: locating the failure point of the sample by the failure location method as described above;

[0070] Step S20: performing accelerated voltage observation on the failure point through SEM; or, preparing TEM samples and performing observation to analyze the failure mechanism.

[0071] It should be noted that in step S20, HV observation is performed on the failure point of the sample by means of a SEM machine, or a TEM (Transmission Electron Microscope) machine is used to prepare a TEM sample and the morphology of the TEM sample is observed, so as to analyze and obtain the corresponding failure mechanism.

[0072] In summary, in the test structure, failure location method and failure analysis method provided in the embodiments of the present invention, the test structure includes: a comb structure, a metal connection and a plurality of semiconductor structures; the semiconductor structure includes: a well region, an active region and a plurality of gates arranged on the well region, and the plurality of gates are arranged at intervals along a first direction; the plurality of semiconductor structures are arranged at intervals along a second direction, and in two adjacent semiconductor structures, the active region and the plurality of gates in one semiconductor structure are connected in sequence through a metal connection; the active region and the plurality of gates in the other semiconductor structure are connected to the metal connection one-to-one, and the one-to-one corresponding metal connections are independent of each other; the comb structure is connected to the semiconductor structure through a metal connection.

[0073] In such a configuration, an active area and multiple gates in a semiconductor structure are sequentially connected by metal wiring, so that in the voltage contrast image, a first through hole located above the corresponding semiconductor structure is highlighted, while in another semiconductor structure adjacent thereto, the metal wiring is connected to the active area and multiple gates in a one-to-one correspondence, and in the voltage contrast image, the first through hole located above the corresponding semiconductor structure is dark. Therefore, by arranging the connection methods of the above two different metal wirings at intervals, the difference in brightness can be seen in the voltage contrast image, and the abnormal failure point can be quickly located, thereby improving the efficiency of failure location, and at the same time, it is not easy to miss small-size defects, further improving the accuracy of failure location.

[0074] Furthermore, by using the above-mentioned test structure, the operator only needs to search for the first through hole with abnormal light and dark states in the voltage contrast image to determine that the corresponding position in the semiconductor structure below the first through hole is the failure point. It is no longer necessary to search over a large area in the hot spot area, which improves the efficiency of failure analysis while making it less likely to miss small-sized defects, further improving the accuracy of failure analysis.

[0075] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A test structure, characterized in that: include: Comb structures, metal interconnects, and multiple semiconductor structures; The semiconductor structure comprises: a well region, an active region and a plurality of gates disposed on the well region, wherein the plurality of gates are arranged at intervals along a first direction; The plurality of semiconductor structures are arranged at intervals along the second direction. In two adjacent semiconductor structures, the active region and the plurality of gates in one semiconductor structure are sequentially connected through one metal wire; the active region and the plurality of gates in the other semiconductor structure are connected to the metal wire in a one-to-one correspondence, and the one-to-one corresponding metal wires are independent of each other. The comb-shaped structure is connected to the semiconductor structure through the metal wiring.

2. The test structure according to claim 1, characterized in that The test structure includes a first interconnect structure and a second interconnect structure; The first interconnect structure is formed by sequentially connecting the active region and the plurality of gates in one of the semiconductor structures with the metal wires; The second interconnect structure is formed by connecting the metal wires with the active region and the plurality of gates in one semiconductor structure in a one-to-one correspondence; The first interconnect structures and the second interconnect structures are alternately arranged along the second direction.

3. The test structure according to claim 2, characterized in that: The test structure includes a first through hole and two comb-shaped structures. The first through hole is arranged in one-to-one correspondence with the gate, and the two comb-shaped structures are respectively connected to the first interconnection structure and the second interconnection structure through the first through hole.

4. The test structure according to claim 3, characterized in that: The comb-like structure comprises a comb back and a plurality of comb teeth, wherein the comb teeth extend along the first direction, the plurality of comb teeth are arranged at intervals along the second direction, and the comb back is sequentially connected to one end of the plurality of comb teeth; The comb teeth of one of the comb-like structures are connected to the first interconnection structures in a one-to-one correspondence; the comb teeth of the other comb-like structure are connected to the second interconnection structures in a one-to-one correspondence.

5. The test structure according to claim 4, characterized in that: The comb-like structure also includes a second through hole, which is arranged on one side of the comb teeth. The comb teeth are connected to the comb back through the second through hole, and the second through holes in the same comb-like structure are located on the same side of the comb teeth.

6. The test structure according to claim 4, characterized in that: The comb teeth include a first metal layer; the comb back includes a second metal layer.

7. The test structure according to claim 1, characterized in that: The first direction and the second direction are perpendicular to each other.

8. A failure location method, characterized in that: include: Providing a sample comprising a test structure as claimed in any one of claims 1 to 7, wherein the sample comprises a failure point; Obtaining a hot spot area of ​​the sample, wherein the failure point is located in the hot spot area; Grinding the sample to the first through-hole layer, and performing voltage contrast observation on the sample to obtain a voltage contrast image; The voltage contrast image is observed to compare the brightness difference of the first through hole to locate the failure point.

9. The failure location method according to claim 8, characterized in that: The sample includes a first interconnect structure and a second interconnect structure; The first through hole located above the first interconnect structure is in a highlighted state in the voltage contrast image; the first through hole located above the second interconnect structure is in a dark state in the voltage contrast image; The step of observing the voltage contrast image and comparing the light and dark difference of the first through hole to locate the failure point comprises: If the first through hole located above the second interconnect structure is highlighted in the voltage contrast image, the failure point is a position corresponding to the first through hole in the second interconnect structure.

10. A failure analysis method, characterized in that: include: Locating the failure point of the sample by the failure location method according to any one of claims 8 to 9; Performing accelerated voltage observation on the failure point by SEM; or, TEM samples were prepared and observed to analyze the failure mechanism.

Citation Information

Cited By

  • Semiconductor LDD extension width test structure and forming method and calculation method thereof

    CN119381387A